Materials Algorithms Project
FORTRAN Library
Program MAP_STEEL_MO2C
-
Provenance of code.
-
Purpose of code.
-
Specification.
-
Description of subroutine's operation.
-
References.
-
Parameter descriptions.
-
Error indicators.
-
Accuracy estimate.
-
Any additional information.
-
Example of code
-
Auxiliary subroutines required.
-
Keywords.
-
Download source code.
-
Links.
Provenance of Source Code
Nobuhiro FUJITA and H. K. D. H. Bhadeshia
Phase Transformations Group,
Department of Materials Science and Metallurgy,
University of Cambridge,
Cambridge, U.K.
Top | Next
Purpose
To calculate the kinetics of the diffusion-controlled precipitation of carbides (taking capillarity effects into account), with particular reference to the carbides
in secondary hardening steels (Fe-Mo-C steel). It is assumed that the first carbide to form is cementite.
Top | Next | Prev
Specification
This is a self-contained program.
Top | Next | Prev
Description
The program reads thermodynamic data (e.g. from MTDATA or Thermocalc) from
a pre-established database. It then calculates the evolution of volume
fraction and particle size with time for up to 4 carbides forming simultaneously.
Top | Next | Prev
References
-
N. Fujita and H. K. D. H. Bhadeshia, 'Precipitation of Molybdenum Carbide
in Steel: Multicomponent-Diffusion & Multicomponent Capillarity', Materials Science and Technology, 1998, in press.
-
J. D. Robson and H. K. D. H. Bhadeshia, 'Simultaneous Kinetics in Power
Plant Steels: Part 1 - Kinetic Theory', Materials Science and Technology, 13
(8) 631-639 1997.
Top | Next | Prev
Parameters
Input parameters
-
TK - double precision
-
Temperature in K.
-
DG - double precision array of size 4
-
Driving force for formation of carbides 1-4.
-
XB - double precision array of size 4
-
Mean composition of species 1-4 (mole fraction).
-
XC - double precision array of size 4x4
-
Equilibrium composition of species 1-4 in carbides 1-4 (mole fraction).
-
XA - double precision array of size 4x4
-
Composition of species 1-4 matrix in equilibrium with carbides 1-4 (mole
fraction).
-
CXB - double precision array of size 4
-
Mean carbon composition of species 1-4 (mole fraction).
-
CXC - double precision array of size 4x4
-
Equilibrium carbon composition of species 1-4 in carbides 1-4 (mole fraction).
-
CXA - double precision array of size 4x4
-
Carbon composition of species 1-4 matrix in equilibrium with carbides 1-4
(mole fraction).
-
VMAX - double precision array of size 4
-
Maximum volume fraction of carbides 1-4.
-
SFEN - double precision array of size 4
-
Interfacial energy for nuclei of carbides 1-4 (Jm-2).
-
NAD - double precision array of size 4
-
Nucleation site density factor for carbides 1-4.
-
CTYPE - double precision array of size 4
-
Morphology for carbides 1-4.
-
1 = Needle shaped
-
2 = Spherical
-
DS - double precision array of size 4
-
Species assumed to be controlling growth for phase 1-4.
-
CC - double precision
-
Mean carbon concentration (wt%).
-
GTHI - double precision
-
Thickness of cementite on boundaries (m).
-
THI - double precision
-
Thickness of cementite within grain (m).
-
DR - double precision array of size 4
-
The ratio of cementite density between on boundaries and with in grains.
Output parameters
T - double precision
Time in seconds.
-
VE - double precision array of size 4
-
Volume fraction of carbides 1-4.
-
SZEX - double precision array of size 4x the number of time steps
-
The particle size for carbides 1-4.
Top | Next | Prev
Error Indicators
None.
Top | Next | Prev
Accuracy
No information supplied.
Top | Next |
Prev
Further Comments
The program is set to read the input data from an ASCII text file 'datain.d'
and to write the results to file 'dataout.d'. An sample version of 'datain.d'
is provided.
Top | Next | Prev
Example
An example for cementite and Mo2C precipitating in a ternary Fe-2wt%Mo-0.1wt%C
steel.
1. Program text
Complete program
2. Program data
0
0.0D0
1.0D0
0.0D0
1.0D0
0.18623d-1
0.0D0
0.0D0
0.18623d-1
0.0114
0.061498
0.010433
0.00514
0.25
0.000493
0.2481
1d-6
1.0D0
1.0D0
0.150d-1
0.150d-1
-1.29d2
0.150d-1
0.0114
0.582579
0.001192
0.00514
0.33
0.000493
50
923
0.11
0.9
5D-8
2D-8
3. Program results
Time/s Vol.F.(Cem.) Mo2C Vol.F. Mo2C Max.Size/m
0.10000D+03 0.18623D-01 0.12689D-09 0.41117D-08
0.15000D+03 0.18623D-01 0.49499D-09 0.61235D-08
0.20000D+03 0.18623D-01 0.13401D-08 0.81058D-08
0.25000D+03 0.18623D-01 0.29375D-08 0.10058D-07
0.30000D+03 0.18623D-01 0.56070D-08 0.11981D-07
0.35000D+03 0.18623D-01 0.97042D-08 0.13875D-07
0.40000D+03 0.18623D-01 0.15612D-07 0.15738D-07
0.45000D+03 0.18623D-01 0.23733D-07 0.17571D-07
0.50000D+03 0.18623D-01 0.34481D-07 0.19374D-07
0.55000D+03 0.18623D-01 0.48276D-07 0.21147D-07
0.60000D+03 0.18623D-01 0.65536D-07 0.22890D-07
0.65000D+03 0.18623D-01 0.86671D-07 0.24602D-07
0.70000D+03 0.18623D-01 0.11208D-06 0.26284D-07
0.75000D+03 0.18623D-01 0.14214D-06 0.27935D-07
0.80000D+03 0.18623D-01 0.17720D-06 0.29555D-07
0.85000D+03 0.18623D-01 0.21760D-06 0.31145D-07
0.90000D+03 0.18623D-01 0.26363D-06 0.32704D-07
0.95000D+03 0.18623D-01 0.31559D-06 0.34232D-07
0.10000D+04 0.18623D-01 0.37429D-06 0.35744D-07
0.10500D+04 0.18623D-01 0.44018D-06 0.37240D-07
0.11000D+04 0.18623D-01 0.51367D-06 0.38720D-07
0.11500D+04 0.18623D-01 0.59519D-06 0.40184D-07
0.12000D+04 0.18623D-01 0.68513D-06 0.41632D-07
0.12500D+04 0.18623D-01 0.78388D-06 0.43063D-07
0.13000D+04 0.18623D-01 0.89181D-06 0.44479D-07
0.13500D+04 0.18623D-01 0.10093D-05 0.45878D-07
0.14000D+04 0.18623D-01 0.11366D-05 0.47261D-07
0.14500D+04 0.18623D-01 0.12741D-05 0.48628D-07
0.15000D+04 0.18623D-01 0.14221D-05 0.49979D-07
0.15500D+04 0.18623D-01 0.15808D-05 0.51313D-07
0.16000D+04 0.18623D-01 0.17506D-05 0.52631D-07
0.16500D+04 0.18623D-01 0.19315D-05 0.53932D-07
0.20500D+04 0.18623D-01 0.38009D-05 0.63757D-07
0.26000D+04 0.18623D-01 0.76084D-05 0.75582D-07
0.32500D+04 0.18623D-01 0.14102D-04 0.87807D-07
0.40500D+04 0.18623D-01 0.26060D-04 0.10179D-06
0.51000D+04 0.18623D-01 0.50134D-04 0.11895D-06
0.64000D+04 0.18623D-01 0.98992D-04 0.13963D-06
0.80000D+04 0.18623D-01 0.20007D-03 0.16459D-06
0.10050D+05 0.18623D-01 0.41993D-03 0.19565D-06
0.12650D+05 0.18594D-01 0.88711D-03 0.23315D-06
0.15900D+05 0.18383D-01 0.18181D-02 0.27660D-06
0.20050D+05 0.17502D-01 0.35586D-02 0.32586D-06
0.25200D+05 0.14879D-01 0.62906D-02 0.37594D-06
0.31700D+05 0.88666D-02 0.97735D-02 0.42109D-06
0.39900D+05 0.00000D+00 0.12033D-01 0.44464D-06
0.50200D+05 0.00000D+00 0.12632D-01 0.45037D-06
0.63150D+05 0.00000D+00 0.13115D-01 0.45486D-06
0.79500D+05 0.00000D+00 0.13500D-01 0.45835D-06
0.10005D+06 0.00000D+00 0.13803D-01 0.46105D-06
0.12595D+06 0.00000D+00 0.14040D-01 0.46313D-06
0.15855D+06 0.00000D+00 0.14225D-01 0.46475D-06
0.19960D+06 0.00000D+00 0.14370D-01 0.46600D-06
0.25125D+06 0.00000D+00 0.14483D-01 0.46697D-06
0.31630D+06 0.00000D+00 0.14572D-01 0.46773D-06
0.39820D+06 0.00000D+00 0.14641D-01 0.46832D-06
0.50125D+06 0.00000D+00 0.14695D-01 0.46878D-06
0.63105D+06 0.00000D+00 0.14738D-01 0.46914D-06
0.79440D+06 0.00000D+00 0.14772D-01 0.46942D-06
Top | Next | Prev
Auxiliary Routines
The subroutines called by this program are :-
CONST
GROWTH
LINEARGROWTH
PARABOLGROWTH
SIZE
NURATE
DIFCO
USER
LINECALC
Top | Next | Prev
Keywords
simultaneous precipiateion reactions, capillarity, secondary hardening
steel
Top | Next | Prev
Download
Download source code
Top | Prev
MAP originated from a joint project of the National Physical
Laboratory and the University of Cambridge.
MAP Website administration / map@msm.cam.ac.uk
Top | Index
| MAP Homepage