Date and time of run 15-JAN-2007 10:56:42 > 20070115104656 MTDATA 4.74 2004-11-18 12:00, LOG D:\MTDATA\Work\mt47.log > 20070115104656 user2 on DVF-400-* using D:\MTDATA\DVF\mtdata.exe > 20070115105640 MODULE 3 creates MPI file D:\MTDATA\Work\def.mpi > 20070115105642 MODULE 3 reads MPI file D:\MTDATA\Work\def.mpi > 20070115105642 MODULE 3 creates MPR file D:\MTDATA\Work\def.mpr $(Number of lines of title) 8 * DATAFILE = D:\MTDATA\Work\def.mpi - CREATED 10:56:40 15-JAN-2007 * SYSTEM = C,Mn,Ni,Fe, * NUMBER OF PHASES = 23 * NUMBER OF SPECIES = 81 * DATA FILE = D:\MTDATA\Work\def.mpi *** PROBLEM settings *** SYSTEM ELEMENTS : CFeMnNi NUMBER COMPONENT STATUS AMOUNT DELTA REF.P 1 C NORMAL 10.9316 2 Mn #PARA! 41.4103 3 Ni #PARA! 68.7170 4 Fe # TO BAL 1675.30 NUMBER PHASE STATUS MODEL 1 DIAMOND_A4 absent PURE SUBSTANCE 2 GRAPHITE absent PURE SUBSTANCE 3 LIQUID absent REDLICH-KISTER 4 BCC_A2 NORMAL SUBLATTICE 5 CBCC_A12 absent SUBLATTICE 6 CEMENTITE absent SUBLATTICE 7 CUB_A13 absent SUBLATTICE 8 FCC_A1 absent SUBLATTICE 9 FE4N absent SUBLATTICE 10 FECN_CHI absent PURE SUBSTANCE 11 HCP_A3 absent SUBLATTICE 12 KSI_CARBIDE absent PURE SUBSTANCE 13 M3C2 absent SUBLATTICE 14 M5C2 absent SUBLATTICE 15 M7C3 absent SUBLATTICE 16 V3C2 absent SUBLATTICE 17 M23C6 absent SUBLATTICE 18 AL5FE4 absent REDLICH-KISTER 19 ORTHORHOMBIC_A20 absent PURE SUBSTANCE 20 TETRAGONAL_U absent PURE SUBSTANCE 21 LAVES_C14 absent SUBLATTICE 22 LAVES_C15 absent SUBLATTICE 23 BCC_B2 absent CHEMICAL ORDERING(C) NUMBER SUBSTANCE STATUS/CONSTRAINT 1 C NORMAL 2 C NORMAL 3 C NORMAL 4 Fe NORMAL 5 Mn NORMAL 6 Ni NORMAL 7 Fe:1 NORMAL 8 Mn:1 NORMAL 9 Ni:1 NORMAL 10 C:2 NORMAL 11 Va:2 NORMAL 12 Fe:1 NORMAL 13 Mn:1 NORMAL 14 Ni:1 NORMAL 15 C:2 NORMAL 16 Va:2 NORMAL 17 Fe:1 NORMAL 18 Mn:1 NORMAL 19 Ni:1 NORMAL 20 C:2 NORMAL 21 Fe:1 NORMAL 22 Mn:1 NORMAL 23 Ni:1 NORMAL 24 C:2 NORMAL 25 Va:2 NORMAL 26 Fe:1 NORMAL 27 Mn:1 NORMAL 28 Ni:1 NORMAL 29 C:2 NORMAL 30 Va:2 NORMAL 31 Fe:1 NORMAL 32 Mn:1 NORMAL 33 Ni:1 NORMAL 34 C:2 NORMAL 35 Va:2 NORMAL 36 Fe5C2 NORMAL 37 Fe:1 NORMAL 38 Mn:1 NORMAL 39 Ni:1 NORMAL 40 C:2 NORMAL 41 Va:2 NORMAL 42 Fe3C NORMAL 43 Fe:1 NORMAL 44 Mn:1 NORMAL 45 C:2 NORMAL 46 Fe:1 NORMAL 47 Mn:1 NORMAL 48 C:2 NORMAL 49 Fe:1 NORMAL 50 Mn:1 NORMAL 51 Ni:1 NORMAL 52 C:2 NORMAL 53 Fe:1 NORMAL 54 Mn:1 NORMAL 55 C:2 NORMAL 56 Fe:1 NORMAL 57 Mn:1 NORMAL 58 Ni:1 NORMAL 59 Fe:2 NORMAL 60 Mn:2 NORMAL 61 Ni:2 NORMAL 62 C:3 NORMAL 63 Fe NORMAL 64 Mn NORMAL 65 Fe NORMAL 66 Fe NORMAL 67 Fe:1 NORMAL 68 Mn:1 NORMAL 69 Ni:1 NORMAL 70 Fe:2 NORMAL 71 Mn:2 NORMAL 72 Ni:2 NORMAL 73 Fe:1 NORMAL 74 Ni:1 NORMAL 75 Fe:2 NORMAL 76 Ni:2 NORMAL 77 Fe:1 NORMAL 78 Ni:1 NORMAL 79 Fe:2 NORMAL 80 Ni:2 NORMAL 81 Va:3 NORMAL UNARY SOURCE Tmin/K Tmax/K C mtsol 298.15 6000.00 C mtsol 298.15 6000.00 C mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Mn mtsol 298.15 2000.00 Ni mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C NODATA 298.15 298.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe5C2 mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe3C mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 6000.00 Fe:Fe:C mtsol 298.15 6000.00 Fe:Mn:C mtsol 298.15 2000.00 Fe:Ni:C mtsol 298.15 3000.00 Mn:Fe:C mtsol 298.15 2000.00 Mn:Mn:C mtsol 298.15 2000.00 Mn:Ni:C NODATA 298.15 298.00 Ni:Fe:C mtsol 298.15 3000.00 Ni:Mn:C NODATA 298.15 298.00 Ni:Ni:C mtsol 298.15 3000.00 Fe mtsol 298.15 6000.00 Mn mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Fe:Fe mtsol 298.15 6000.00 Fe:Mn NODATA 298.15 298.00 Fe:Ni NODATA 298.15 298.00 Mn:Fe NODATA 298.15 298.00 Mn:Mn mtsol 298.15 2000.00 Mn:Ni NODATA 298.15 298.00 Ni:Fe NODATA 298.15 298.00 Ni:Mn NODATA 298.15 298.00 Ni:Ni mtsol 298.15 3000.00 Fe:Fe mtsol 298.15 6000.00 Fe:Ni NODATA 298.15 298.00 Ni:Fe NODATA 298.15 298.00 Ni:Ni mtsol 298.15 3000.00 Fe:Fe:Va mtsol 298.15 6000.00 Fe:Ni:Va NODATA 298.15 298.00 Ni:Fe:Va NODATA 298.15 298.00 Ni:Ni:Va mtsol 298.15 3000.00 TEMPERATURE : 993.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 Stage 1* only requested *** MULTIPHASE - Stage 1* Results *** Temperature = 993.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -7.8650035813E+07 J System Enthalpy = 4.7331524830E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 973.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 973.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -7.6133358211E+07 J System Enthalpy = 4.5304535587E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 953.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 953.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -7.3658132822E+07 J System Enthalpy = 4.3335312353E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 933.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 933.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -7.1223238873E+07 J System Enthalpy = 4.1457884107E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 913.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 913.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -6.8827700813E+07 J System Enthalpy = 3.9660797426E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 893.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 893.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -6.6470728222E+07 J System Enthalpy = 3.7934616268E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 873.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 873.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -6.4151687602E+07 J System Enthalpy = 3.6271532574E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 853.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 853.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -6.1870079621E+07 J System Enthalpy = 3.4665052180E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 833.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 833.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -5.9625520836E+07 J System Enthalpy = 3.3109741799E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 813.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 813.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -5.7417729112E+07 J System Enthalpy = 3.1601025672E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 793.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 793.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -5.5246512103E+07 J System Enthalpy = 3.0135022311E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 773.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 773.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -5.3111758254E+07 J System Enthalpy = 2.8708413674E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 753.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 753.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -5.1013429912E+07 J System Enthalpy = 2.7318340372E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 733.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 733.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -4.8951558193E+07 J System Enthalpy = 2.5962317882E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 713.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 713.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -4.6926239340E+07 J System Enthalpy = 2.4638169575E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 693.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 693.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -4.4937632348E+07 J System Enthalpy = 2.3343973248E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 673.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 673.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -4.2985957700E+07 J System Enthalpy = 2.2078018507E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 653.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 653.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -4.1071497082E+07 J System Enthalpy = 2.0838772820E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 633.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 633.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -3.9194593992E+07 J System Enthalpy = 1.9624854634E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 613.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 613.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -3.7355655180E+07 J System Enthalpy = 1.8435012118E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 593.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 593.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -3.5555152895E+07 J System Enthalpy = 1.7268106554E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 573.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 573.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 BCC_A2 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 BCC_A2 0.9326089 Gibbs Energy = -3.3793627923E+07 J System Enthalpy = 1.6123099558E+07 J