Bainite, martensite and retained austenite

Study guide, by H. K. D. H. Bhadeshia

Material Data:
Composition: Fe-0.2C-2Si-2Mn wt%
Shear modulus (\(\mu\)): 80 GPa
Molar volume of iron: \(\approx 7 \times 10^{-6} \text{ m}^3\text{mol}^{-1}\)
Strain energy per unit volume: \(\frac{c}{r}\mu (s^2+\delta^2)\)
Figure 1
T0 Curve Diagram

\( T_0 \) curve for Fe-0.2C-2Si-2Mn wt%

a. Describe an experiment to establish if carbon diffuses during bainite growth.
The \( T_0 \) curve describes the locus of points on a temperature versus carbon concentration plot, where austenite and ferrite with the same free energy have identical composition. Therefore, if the carbon concentration \( x_\gamma \) of the austenite exceeds \( x_{T_0} \) (the value given by the \( T_0 \) curve), then diffusionless transformation is impossible.

Thus, if the bainite reaction stops when the \( x_\gamma = x_{T_0} \) then the growth is diffusionless. On the other hand, equilibrium transformation with the partitioning of carbon can continue until \( x_\gamma = x_{\gamma\alpha} \), where \( x_{\gamma\alpha} \) is given by the \( \alpha+\gamma/\gamma \) phase boundary on the equilibrium phase diagram (also called the \( Ae3 \) curve in steel jargon).

One complication is that the strain energy of transformation should be taken into account in calculating the \( T_0 \) curve.
b. A particular steel has the chemical composition Fe-0.2C-2Si-2Mn wt%, the \(T_0\) curve of which is presented below. Beginning with the fully austenitic state, it is transformed isothermally to bainite at 400\(^\circ\)C until the reaction stops. Calculate the volume fractions of the phases present, and the carbon concentration of the austenite when the reaction ceases. Comment on the role of the silicon and state any assumptions involved in your calculation.
At 400°C, the reaction will stop when \( x_\gamma = x_{T_0} \), which from the diagram (Figure 1) gives \( x_\gamma = 0.8 \) wt%.

Using mass balance: \[ \overline x = V_\gamma x_\gamma + (1-V_\gamma) x_\alpha \] where:
  • \( \overline x = 0.2 \) wt% (average concentration)
  • \( V_\gamma \) is the volume fraction of austenite
  • \( x_\alpha \approx 0 \) (carbon concentration in bainitic ferrite after dumping)
Calculation: \[ 0.2 = V_\gamma(0.8) + (1-V_\gamma)(0) \] \[ V_\gamma = 0.2 / 0.8 = 0.25 \]
Result: Volume fraction of austenite is 0.25 and ferrite is 0.75.

Comment on Silicon: The concentration of silicon in the alloy prevents cementite precipitation, making the mass balance equation involving just austenite and ferrite feasible.
c. Describe what happens upon cooling to ambient temperature.
If the martensite-start temperature of the austenite left (taking account of its enriched carbon concentration) is greater than the ambient temperature, then some martensite will form from the residual austenite.
d. Calculate the maximum thickness of martensite plates (austenite grain size = 40 μm).
By balancing the elastic strain energy per unit volume against the driving force for transformation, and assuming \( r = 40 \) μm (the grain size), \(s\) and \(\delta\) are the shear and dilatational strains associated with the invariant-plane strain shape deformation. \(c\) and \(r\) are the thickness and length, respectively, of the plate: \[ \frac{c}{r}\mu (s^2+\delta^2) = \frac{1000 \text{ J mol}^{-1}}{7 \times 10^{-6} \text{ m}^3\text{mol}^{-1}} \] \[ c = \frac{1000 \times 40 \times 10^{-6}}{80 \times 10^9 \times (0.26^2 + 0.03^2) \times 7 \times 10^{-6}} \]
Result: \( c = 1.04 \) μm.
e. Compare bainite plate thickness versus martensite plate thickness.
Plates of martensite are only stopped by the austenite grain boundaries or other plates, so it is reasonable that the coarsest plates will have the same length as the austenite grain size.

However, the bainite plates grow to a limited size of about 10 μm even when they do not collide with any hard barriers. This is because the shape deformation is at high temperatures accommodated plastically, and the resulting dislocation debris kill the growth of the plate once there is a sufficiently large dislocation density.