Provenance of Source Code
Carlos Capdevila, Francisca G. Caballero and Carlos Garcia de Andres,
Phase TRansformation group (GITFES),
Department of
Physical Metallurgy,
National Center for Metallurgical Research (CENIM),
Madrid, Spain.
The neural network program was produced by:
David MacKay,
Cavendish Laboratory,
University of Cambridge,
Madingley Road,
Cambridge, CB3 0HE, U.K.
Added to MAP: August 2000
Top
| Next
Purpose
Estimation of the Ms temeprature in steels as a function of
chemical composition and previous austenite grain size (PAGS).
Top
| Next
| Prev
Specification
| Language: |
FORTRAN / C |
| Product form: |
Source code / Executable files |
| Operating Selntem: |
Windows 95/98/2000 |
Top
| Next
| Prev
Description
MAP_STEEL_MS-TEMPERATURE
contains a suite of programs which enable the user to estimate the Ms temperature as a
function of chemical composition and previous austenite grain size. It makes use of
a neural network program called generate44, which was developed
by David MacKay and is part of the bigback5 program. The network
was trained using a large database of experimental results [1].
16 different models are provided, which differ from each other by the number of
hidden units and by the value of the seed used when training the network. It was
found that a more accurate result could be obtained by averaging the results
from all the models [1].
This suite of programs calculates the results of each model and then combines
them, by averaging, to produce a committee result and error estimate, as
described by MacKay [page
387 of reference 2]. The source code for the neural network program can be
downloaded from David MacKay's
website; the executable files only are available from MAP. Also provided are
FORTRAN programs (as source code) for normalising the input data, averaging the
results from the neural network program and unnormalising the final output file,
along with other files necessary for running the program.
Programs are available which run on a PC under Windows 95/98/2000. A set of program and data files are
provided for the model, which calculate the Ms temperature in steels.
The files for PC are included in a directory called MS_files. This
directory contains the following files and subdirectories:
- README
- A text file containing step-by-step instructions for running the program,
including a list of input variables.
- MINMAX
- A text file containing the minimum and maximum limits of each input and
output variable. This file is used to normalise and unnormalise the input and
output data.
- test.dat
- An input text file containing the input variables used for predictions.
- MS.exe
- This executable program for the PC.
- norm_test.in
- This is a text file which contains the normalised input variables. It is
generated by the program MS.exe.
- generate44
- This is the executable file for the neural network program.
- It reads the normalised input data file and uses the weight files in subdirectory
c. The results are written to the temporary output file
_out.
- Model_RESULT
- Contains the final un-normalised committee results for the predicted
percentage retained austenite.
- SUBDIRECTORY s
- committee.dat
- A text file containing the number of models to be used to form the
committee result and the number of input variables.
- Log_com
- A text file containing information about number of input variables and weight file for committee models.
- SUBDIRECTORY c
- _w*f
- The weights files for the different models.
- *.lu
- Files containing information for calculating the size of the error bars
for the different models.
- _c*
- Files containing information about the perceived significance value [1]
for each model.
- _R*
- Files containing values for the noise, test error and log predictive error
[1]
for each model.
- SUBDIRECTORY d
- outran.x
- A normalised output file which was created during the building of the
model. It is accessed by generate44.
- SUBDIRECTORY outprdt
- out1, out2 etc.
- The normalised output files for each model.
- com.dat
- The normalised output file containing the committee results. It is
generated by gencom.for.
Detailed instructions on the use of the program are given in the README
files. Further information about this suite of programs can be obtained from
reference 1.
Top
| Next
| Prev
References
- C. Capdevila, F.G. Caballero and C. Garcia de Andres, Prediction of Ms Temperature in Steels Submitted to
Materials Science and Technology, 2002.
- D.J.C. MacKay, 1997, Mathematical Modelling of Weld Phenomena 3,
eds. H. Cerjak & H.K.D.H. Bhadeshia, Inst. of Materials, London, pp 359.
- D.J.C MacKay's website at
http://wol.ra.phy.cam.ac.uk/mackay/README.html#Source_code
Top
| Next
| Prev
Parameters
Input parameters
The input variables for the model are listed in the
README.DOC file in the corresponding directory.
The maximum and minimum values for each variable are given in the file
MINMAX.
Output parameters
These program gives the Ms temperature in 'K'. The corresponding output files is called Result.dat or
Result. The format of the output file is: Prediction Error-Bar Upper-limit Lower-limit
(K) (K) (K) (K)
Top
| Next
| Prev
Error Indicators
None.
Top
| Next
| Prev
Accuracy
A full calculation of the error bars is
presented in reference 1.
Top
| Next
| Prev
Further Comments
None.
Top
| Next
| Prev
Example
1. Program text
Complete program.
2. Program data
See sample data file: test.dat.
3. Program results
See sample output file: Result or
Result.dat.
Top
| Next
| Prev
Auxiliary Routines
None
Top
| Next
| Prev
Keywords
neural network, Ms temperature, Steels
Top
| Next
| Prev
Download
Download
Ms temperature Model
Top
| Prev
MAP originated from a joint project of the National Physical
Laboratory and the University of Cambridge.
Top | Index | MAP Homepage