#H S_W[ 1]  S_W[ 2]  S_W[ 3]  S_W[ 4]  S_W[ 5]  S_W[ 6]  S_W[ 7]  S_W[ 8]  S_W[ 9]  S_W[10]  S_W[11]  S_W[12]  S_W[13]  S_W[14]  S_W[15]  S_W[16]  S_W[17]  S_W[18]  S_W[19]  S_W[20]  S_W[21]  S_W[22]  S_W[23]  SIGMA_NU D_EN    D_X2 /NDF WX2/k1 WX2/k2 WX2/k3 WX2/k4 WX2/k5 WX2/k6 WX2/k7 WX2/k8 WX2/k9 WX2/k10 WX2/k11 WX2/k12 WX2/k13 WX2/k14 WX2/k15 WX2/k16 WX2/k17 WX2/k18 WX2/k19 WX2/k20 WX2/k21 WX2/k22 WX2/k23 GAMMA3 LOGOC3  LOGOCF  SYMS NU T_EN   MT_EB     T_X2   NDF  T_EN 2   MT_E2B   T_X2 2 NDF  EVAB    EVB     EVDENCE EVAB2   FUDGE1  FUDGE2  
7  20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       0.3      0.7234  16.07 920 0.05714 0.09442 0.1017 0.03012 0.08028 0.1112 0.0599 0.07254 0.01107 0.07756 0.06698 0.03312 0.07418 0.02478 0.05424 0.06144 1.042  0.503  1.027  0.1171 1.009  0.3523 0.01263 136.5  224.2   -634.2  32   0  0.72335  192.78   16.07  920 0.72335  192.78   16.07  920 -370.25 -419.72 -423.4  -146.09 0.014137 481.76  
7  2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    0.3      0.7233  16.07 920 3.119  5.155  5.552  1.645  4.383  6.072  3.27   3.96   0.6045 4.234  3.657  1.808  4.049  1.353  2.961  3.354  56.89  27.46  56.05  6.39   55.1   19.23  0.6897 93.03  135.8   -310.2  1    0  0.72331  211.17   16.07  920 0.72331  211.17   16.07  920 -52.304 -97.054 -100.76 83.506  0.0098866 333.5   
7  0.6212   0.7693   0.8632   0.4225   0.7025   0.9602   0.6507   0.7024   0.3663   0.6676   0.7783   0.428    0.7012   0.4458   0.7463   0.6222   3.035    2.456    2.943    0.8851   2.576    1.579    0.3663   0.041825 0.4272  488.4 920 90.45  38.52  5.881  52.41  110.3  47.38  65.91  34.86  2.318  16.96  9.21   5.59   40.52  46.1   37.81  20.62  49.03  112.6  17.04  101.3  25.03  86.9   408.4  134.1  133.9   -119.9  1    0  0.42722  1798.4   488.4  920 0.42722  1798.4   488.4  920 1672.3  1623.1  1619.4  1806.1  0.0007194 946.12  
7  0.6458   0.4948   0.2173   0.3393   0.7874   0.7136   0.5701   0.443    0.0852   0.2845   0.2842   0.1086   0.4785   0.3897   0.6199   0.3057   2.158    2.847    1.236    0.9463   1.293    1.54     0.8741   0.032973 0.3835  705.4 920 64.75  44.03  22.63  10.38  109.4  26.22  43.74  85.89  5.885  86.07  37.53  74.65  125.3  51.33  25.41  66.39  33.23  106.1  36.93  48.97  44.65  48.82  490.4  136    133.9   -52.73  1    0  0.38348  1921.2   705.4  920 0.38348  1921.2   705.4  920 1840    1790.9  1787.2  1973.9  0.00057761 1169.6  
7  0.5333   0.3374   0.1159   0.1139   0.8446   0.3829   0.3875   0.4352   0.03999  0.2763   0.2386   0.1146   0.558    0.3193   0.3806   0.2769   1.252    3.129    0.7715   0.6702   0.8676   1.094    2.28     0.031278 0.3761  768.8 920 66.41  65.51  27.02  13.89  94.7   41.96  41.08  82.29  7.645  47.56  35.43  41.77  59.8   48.51  38.85  64.21  69.2   95.62  57.26  62.03  61.13  62.43  302.9  136.4  133.9   -12.82  1    0  0.37606  1942.2   768.8  920 0.37606  1942.2   768.8  920 1904.8  1855.7  1852    2038.7  0.0005538 1234.2  
7  0.4437   0.2824   0.07123  0.04806  0.8345   0.2673   0.2554   0.4091   0.02233  0.1973   0.1818   0.08472  0.4401   0.2455   0.2964   0.2443   1.054    3.225    0.6038   0.5359   0.6831   0.8781   4.609    0.030981 0.3817  795.3 920 62.91  66.56  36.89  18.97  75.48  49.85  46.58  69.06  10.28  44.47  48.54  46.64  59.99  34.34  37.97  46.5   80.22  91.44  65.4   64.12  73.26  71.49  221.1  134.5  133.9   23.55   1    0  0.38166  1940.3   795.3  920 0.38166  1940.3   795.3  920 1939.4  1890.5  1886.8  2073.3  0.00055517 1254.2  
7  0.3592   0.2383   0.05336  0.02659  0.7337   0.2057   0.1812   0.3498   0.01511  0.1371   0.1618   0.0666   0.3473   0.1601   0.2256   0.1823   0.9554   3.25     0.5065   0.4358   0.5901   0.7562   7.906    0.031173 0.3817  785.5 920 95.97  93.49  65.74  61.89  97.65  84.14  92.5   94.41  22.4   92.12  61.26  75.46  96.34  80.78  65.55  83.5   97.64  90.06  92.96  96.97  98.16  96.4   75.16  130.5  133.9   56.08   1    0  0.38166  1939.7   785.5  920 0.38166  1939.7   785.5  920 1954.8  1906.4  1902.7  2088.6  0.00055271 1230.8  
7  0.3615   0.24     0.05665  0.0309   0.7347   0.2101   0.1854   0.3516   0.01668  0.141    0.1619   0.06914  0.3502   0.1711   0.2333   0.189    0.9562   3.247    0.512    0.4383   0.5918   0.7577   7.174    0.031094 0.3817  789.5 920 94.75  92.17  58.32  45.84  97.38  80.69  88.41  93.48  18.36  87.04  61.18  70.02  94.73  70.68  61.3   77.66  97.49  90.24  90.96  95.85  97.61  96.02  91.28  131.1  133.9   52.62   1    0  0.38166  1940.1   789.5  920 0.38166  1940.1   789.5  920 1953.6  1905.1  1901.4  2087.5  0.00055268 1237    
7  0.3616   0.24     0.05585  0.02956  0.7348   0.2099   0.1851   0.3516   0.01619  0.1407   0.1624   0.06868  0.3502   0.169    0.2322   0.1881   0.9564   3.247    0.5117   0.4383   0.592    0.7579   7.254    0.031107 0.3817  788.9 920 94.71  92.14  60     50.1   97.34  80.84  88.66  93.46  19.49  87.44  60.81  70.97  94.75  72.44  61.85  78.42  97.46  90.22  91.07  95.85  97.53  95.96  89.26  131    133.9   53.35   1    0  0.38166  1940.1   788.9  920 0.38166  1940.1   788.9  920 1954    1905.5  1901.8  2087.9  0.00055265 1235.9  

