#H S_W[ 1]  S_W[ 2]  S_W[ 3]  S_W[ 4]  S_W[ 5]  S_W[ 6]  S_W[ 7]  S_W[ 8]  S_W[ 9]  S_W[10]  S_W[11]  S_W[12]  S_W[13]  S_W[14]  S_W[15]  S_W[16]  S_W[17]  S_W[18]  S_W[19]  S_W[20]  S_W[21]  S_W[22]  S_W[23]  SIGMA_NU D_EN    D_X2 /NDF WX2/k1 WX2/k2 WX2/k3 WX2/k4 WX2/k5 WX2/k6 WX2/k7 WX2/k8 WX2/k9 WX2/k10 WX2/k11 WX2/k12 WX2/k13 WX2/k14 WX2/k15 WX2/k16 WX2/k17 WX2/k18 WX2/k19 WX2/k20 WX2/k21 WX2/k22 WX2/k23 GAMMA3 LOGOC3  LOGOCF  SYMS NU T_EN   MT_EB     T_X2   NDF  T_EN 2   MT_E2B   T_X2 2 NDF  EVAB    EVB     EVDENCE EVAB2   FUDGE1  FUDGE2  
9  20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       0.3      0.5716  12.7  920 0.1278 0.09002 0.09428 0.06284 0.06155 0.05612 0.03434 0.1491 0.0338 0.03127 0.04189 0.092  0.01072 0.2216 0.07342 0.1344 0.3311 0.2019 0.4134 0.1306 1.201  0.1573 0.03436 160.2  350.3   -814.3  180  0  0.57155  184.63   12.7   920 0.57155  184.63   12.7   920 -544.69 -595.91 -599.57 -194.43 0.016289 559.2   
9  2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    0.3      0.5715  12.7  920 6.977  4.915  5.147  3.431  3.361  3.064  1.875  8.141  1.845  1.707  2.287  5.023  0.5855 12.1   4.008  7.338  18.08  11.03  22.57  7.132  65.56  8.586  1.876  101.8  199.5   -398.3  1    0  0.57154  208.98   12.7   920 0.57154  208.98   12.7   920 -132.64 -178.27 -181.97 66.896  0.010581 360.09  
9  1.035    0.8358   0.8909   0.6668   0.653    0.7237   0.5256   1.083    0.6829   0.4427   0.7142   0.806    0.3663   1.526    1.029    1.099    1.776    1.712    1.89     1.066    2.66     1.145    0.3811   0.037377 0.5715  818.2 920 47.7   51.55  47.51  56.53  57.74  42.85  49.72  50.86  28.99  63.84  32.84  56.65  31.96  38.07  27.75  44.47  42.01  27.54  46.29  45.99  67.9   47.99  94.63  132.9  -145.5  -170.2  1    0  0.57152  1755.9   818.2  920 0.57152  1755.9   818.2  920 1568.1  1519.2  1515.5  1422.5  0.00082302 1271.6  
9  0.8486   0.728    0.7518   0.6234   0.6117   0.659    0.5184   0.9044   0.6412   0.4515   0.6651   0.7401   0.304    1.138    0.8144   0.9132   1.329    1.141    1.444    0.8843   2.261    0.9666   0.396    0.038108 0.3252  447.8 920 25.96  61.81  28.22  44.45  76.93  53.32  24.87  35.94  4.662  22.33  9.797  44.63  36.73  12.5   5.929  26.71  42.47  8.512  63.55  28.98  46.96  80.69  350.2  161.5  176.1   -139    1    0  0.32518  1894     447.8  920 0.32518  1894     447.8  920 1763.8  1712.6  1708.9  1939.9  0.00060841 998.96  
9  0.4644   0.6193   0.4291   0.4489   0.5846   0.5729   0.2962   0.5687   0.2092   0.2315   0.2834   0.5274   0.2313   0.4397   0.279    0.5111   0.9196   0.4228   1.22     0.5071   1.563    0.9674   0.9458   0.029282 0.2991  697.7 920 49.65  40.29  33.79  50.33  42.84  68.78  53.28  28.52  5.161  26.34  10.47  34.96  110.2  45.7   12.52  20.46  100.1  7.661  73.49  54.37  56.67  51.92  337.1  170.9  176.1   -47.12  1    0  0.29914  2027.4   697.7  920 0.29914  2027.4   697.7  920 1965.1  1913.4  1909.7  2141.2  0.00048439 1280.8  
9  0.345    0.4046   0.2637   0.3316   0.394    0.5086   0.2385   0.3118   0.07861  0.127    0.1258   0.3206   0.2734   0.3387   0.1591   0.2434   0.9502   0.1558   1.069    0.3897   1.185    0.7144   1.98     0.02826  0.301   753.8 920 52.82  51.16  48.52  26.64  43.02  65.51  49.62  47.93  2.608  51.49  8.02   23.52  55.71  42.39  19.41  20.95  57.43  12.71  86.13  63.04  62.42  74.76  300.9  169.1  176.1   27.15   1    0  0.301    2036.5   753.8  920 0.301    2036.5   753.8  920 2046.4  1995    1991.3  2222.5  0.00047394 1330.7  
9  0.2627   0.2974   0.1965   0.1757   0.266    0.4312   0.1805   0.226    0.02406  0.1007   0.05385  0.16     0.2138   0.2447   0.1182   0.1188   0.7335   0.08909  1.015    0.3212   0.945    0.6303   3.9      0.028314 0.301   750.9 920 91.1   94.69  87.41  94.87  94.4   91.12  86.6   91.25  27.69  82     43.72  94.41  91.06  81.18  35.18  87.91  96.37  38.84  95.54  92.77  98.12  96.04  77.54  160.7  176.1   98.01   1    0  0.301    2037.3   750.9  920 0.301    2037.3   750.9  920 2090.9  2040.5  2036.9  2267    0.00046718 1299.2  
9  0.2666   0.3013   0.2019   0.1832   0.2718   0.4332   0.1853   0.2308   0.03146  0.1024   0.06966  0.1691   0.2171   0.2526   0.1203   0.1321   0.7386   0.1048   1.013    0.3234   0.949    0.6294   3.548    0.028157 0.301   759.3 920 88.48  92.23  82.8   87.29  90.43  90.28  82.2   87.48  16.2   79.21  26.12  84.57  88.35  76.21  33.92  71.06  95.05  28.09  95.95  91.54  97.28  96.33  93.7   162    176.1   88.92   1    0  0.301    2038.5   759.3  920 0.301    2038.5   759.3  920 2086.9  2036.3  2032.6  2263    0.00046682 1312.3  
9  0.2665   0.3013   0.2013   0.1826   0.2715   0.4335   0.1848   0.2305   0.02926  0.1024   0.06338  0.168    0.2169   0.252    0.1216   0.1293   0.7387   0.09922  1.013    0.3235   0.949    0.6299   3.573    0.028182 0.301   758   920 88.53  92.27  83.25  87.84  90.64  90.17  82.66  87.7   18.72  79.26  31.56  85.65  88.49  76.55  33.23  74.24  95.02  31.31  95.85  91.46  97.29  96.18  92.38  161.7  176.1   91.11   1    0  0.301    2038.4   758    920 0.301    2038.4   758    920 2088.3  2037.7  2034.1  2264.4  0.0004668 1309.8  