#H S_W[ 1]  S_W[ 2]  S_W[ 3]  S_W[ 4]  S_W[ 5]  S_W[ 6]  S_W[ 7]  S_W[ 8]  S_W[ 9]  S_W[10]  S_W[11]  S_W[12]  S_W[13]  S_W[14]  S_W[15]  S_W[16]  S_W[17]  S_W[18]  S_W[19]  S_W[20]  S_W[21]  S_W[22]  S_W[23]  SIGMA_NU D_EN    D_X2 /NDF WX2/k1 WX2/k2 WX2/k3 WX2/k4 WX2/k5 WX2/k6 WX2/k7 WX2/k8 WX2/k9 WX2/k10 WX2/k11 WX2/k12 WX2/k13 WX2/k14 WX2/k15 WX2/k16 WX2/k17 WX2/k18 WX2/k19 WX2/k20 WX2/k21 WX2/k22 WX2/k23 GAMMA3 LOGOC3  LOGOCF  SYMS NU T_EN   MT_EB     T_X2   NDF  T_EN 2   MT_E2B   T_X2 2 NDF  EVAB    EVB     EVDENCE EVAB2   FUDGE1  FUDGE2  
12 20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       20       0.3      0.394   8.756 920 0.2073 0.08558 0.09546 0.04093 0.09255 0.08728 0.07311 0.02538 0.02597 0.09779 0.03653 0.03683 0.07777 0.1052 0.0401 0.03391 0.2173 0.05977 0.3128 0.1569 0.8573 0.2812 0.08647 207    469     -1084   13.6 0  0.39403  167.48   8.756  920 0.39403  167.48   8.756  920 -812.04 -866.14 -869.77 -343.09 0.02068 715.15  
12 2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    2.707    0.3      0.394   8.756 920 11.32  4.672  5.212  2.235  5.053  4.765  3.992  1.386  1.418  5.339  1.995  2.011  4.246  5.743  2.19   1.852  11.86  3.263  17.08  8.568  46.81  15.35  4.721  135.4  262.2   -530.4  1    0  0.39401  196.37   8.756  920 0.39401  196.37   8.756  920 -254.49 -303.45 -307.13 7.6788  0.013669 470.61  
12 1.386    0.7971   0.891    0.5209   0.8149   0.9102   0.7587   0.4278   0.6046   0.796    0.6747   0.4741   0.7843   1.083    0.8102   0.5227   1.418    0.8709   1.636    1.13     2.286    1.583    0.6493   0.031691 0.394   784.6 920 43.18  53.87  48.09  60.33  55.74  42.14  50.8   55.47  28.41  61.73  32.1   65.54  50.57  35.85  24.44  49.65  43.25  31.52  46.75  49.16  65.6   44.89  82.03  177.6  239.5   -214.4  1    0  0.39401  1919.5   784.6  920 0.39401  1919.5   784.6  920 1684    1631.9  1628.3  1923.6  0.0006221 1390.5  
12 1.037    0.6906   0.7407   0.505    0.712    0.7508   0.6696   0.4374   0.5907   0.7228   0.6257   0.4852   0.6808   0.8362   0.7299   0.5019   1.08     0.7395   1.263    0.9084   1.958    1.2      0.6539   0.032579 0.2677  504.4 920 69.97  79.92  12.94  15.45  21.6   36.98  22.45  15.95  2.565  29.47  6.992  17.04  38.35  43.02  6.982  13.02  42.14  8.19   55.46  80.73  38.41  49.29  221.1  205.2  239.5   -176.8  1    0  0.2677   2003.9   504.4  920 0.2677   2003.9   504.4  920 1847.2  1793.3  1789.7  2086.8  0.00052773 1204.7  
12 0.9541   0.6801   0.2942   0.2192   0.3565   0.533    0.3549   0.206    0.1543   0.4208   0.2418   0.2276   0.4774   0.6525   0.3015   0.2097   0.7714   0.2807   1.014    0.9004   1.235    0.9241   1.215    0.027368 0.2528  675   920 53.91  71.42  17.25  24.77  27.59  41.46  65.55  33.28  3.055  24.86  15.4   50.72  50.3   28.6   25.97  5.304  46.6   22.6   67.46  36.47  73.95  56.17  277.5  212.4  239.5   -35.05  1    0  0.25281  2092.2   675    920 0.25281  2092.2   675    920 2052.2  1998.1  1994.5  2291.8  0.00044769 1399.6  
12 0.7269   0.5964   0.1377   0.1214   0.2012   0.3762   0.3213   0.1415   0.05016  0.2203   0.1466   0.1879   0.3604   0.3849   0.247    0.05757  0.5589   0.1974   0.862    0.5592   1.074    0.7136   2.442    0.02673  0.2468  690.9 920 47.79  42.49  20.18  34.42  81.11  36.13  58.92  40.48  3.753  30.77  7.465  50.36  69.38  26.71  12.68  9.967  55.11  24.85  78.65  66.07  95.12  67.05  242.3  210.2  239.5   71.34   1    0  0.24684  2107     690.9  920 0.24684  2107     690.9  920 2167.6  2113.7  2110.1  2407.2  0.00043155 1408.2  
12 0.5184   0.3998   0.07456  0.08217  0.2008   0.2455   0.2635   0.1054   0.02093  0.1309   0.06185  0.1485   0.3198   0.2234   0.1226   0.02648  0.4368   0.1429   0.7832   0.4723   1.061    0.5998   4.502    0.026372 0.2468  709.8 920 93.94  94.56  68.87  75.09  81.37  84.87  87.6   72.89  21.54  87.15  41.94  80.62  88.14  79.25  51.46  47.12  90.25  47.4   95.28  92.62  97.53  94.9   71.27  197.9  239.5   163.2   1    0  0.24684  2113.9   709.8  920 0.24684  2113.9   709.8  920 2230.7  2177.9  2174.3  2470.2  0.00041794 1385.2  
12 0.526    0.4083   0.08562  0.08691  0.1975   0.2562   0.2658   0.1099   0.02521  0.1394   0.07709  0.1518   0.3201   0.2411   0.1409   0.03221  0.4426   0.1509   0.7824   0.4736   1.06     0.5982   3.974    0.026148 0.2468  722.1 920 91.24  90.64  52.23  67.12  84.19  77.94  86.08  67.05  14.85  76.91  26.99  77.17  87.96  68.04  38.96  31.83  87.9   42.51  95.46  92.11  97.76  95.4   91.45  200.3  239.5   149.5   1    0  0.24684  2116.2   722.1  920 0.24684  2116.2   722.1  920 2224.9  2171.8  2168.2  2464.4  0.00041715 1405.5  
12 0.5261   0.4079   0.08225  0.08607  0.1983   0.2551   0.266    0.1091   0.02409  0.138    0.07182  0.1514   0.3204   0.2383   0.1363   0.03042  0.4425   0.1492   0.7829   0.474    1.06     0.5992   4.031    0.026191 0.2468  719.7 920 91.22  90.82  56.59  68.44  83.51  78.61  85.96  68.04  16.26  78.41  31.1   77.51  87.81  69.69  41.6   35.68  87.93  43.52  95.34  91.94  97.73  95.1   88.92  199.7  239.5   152.9   1    0  0.24684  2115.8   719.7  920 0.24684  2115.8   719.7  920 2226.7  2173.8  2170.1  2466.3  0.00041723 1401.3  

