#H S_W[ 1]  S_W[ 2]  S_W[ 3]  S_W[ 4]  S_W[ 5]  S_W[ 6]  S_W[ 7]  S_W[ 8]  S_W[ 9]  S_W[10]  S_W[11]  S_W[12]  S_W[13]  S_W[14]  S_W[15]  S_W[16]  S_W[17]  S_W[18]  S_W[19]  S_W[20]  S_W[21]  S_W[22]  S_W[23]  S_W[24]  S_W[25]  S_W[26]  S_W[27]  S_W[28]  S_W[29]  S_W[30]  S_W[31]  S_W[32]  S_W[33]  S_W[34]  S_W[35]  S_W[36]  S_W[37]  S_W[38]  S_W[39]  S_W[40]  S_W[41]  S_W[42]  S_W[43]  S_W[44]  SIGMA_NU D_EN    D_X2 /NDF WX2/k1 WX2/k2 WX2/k3 WX2/k4 WX2/k5 WX2/k6 WX2/k7 WX2/k8 WX2/k9 WX2/k10 WX2/k11 WX2/k12 WX2/k13 WX2/k14 WX2/k15 WX2/k16 WX2/k17 WX2/k18 WX2/k19 WX2/k20 WX2/k21 WX2/k22 WX2/k23 WX2/k24 WX2/k25 WX2/k26 WX2/k27 WX2/k28 WX2/k29 WX2/k30 WX2/k31 WX2/k32 WX2/k33 WX2/k34 WX2/k35 WX2/k36 WX2/k37 WX2/k38 WX2/k39 WX2/k40 WX2/k41 WX2/k42 WX2/k43 WX2/k44 GAMMA3 LOGOC3  LOGOCF  SYMS NU T_EN   MT_EB     T_X2   NDF  T_EN 2   MT_E2B   T_X2 2 NDF  EVAB    EVB     EVDENCE EVAB2   FUDGE1  FUDGE2  
12 42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       42       0.3      1.456   32.35 1976 0.0784 0.2525 0.1528 0.007463 0.02689 0.01699 0.01896 0.0328 0.008776 0.02637 0.05905 0.03506 0.1328 0.01151 0.01342 0.1403 0.06118 0.00969 0.01025 0.01061 0.01194 0.007978 0.03284 0.05729 0.05449 0.03267 0.04213 0.04066 0.0393 0.02755 0.05145 0.01966 0.0347 0.03125 0.0139 0.009899 0.01883 0.01538 0.01674 0.009411 0.01796 0.3923 0.1185 0.005607 252.2  inf     -2463   19.3 0  1.4557   440.04   32.35  1976 1.4557   440.04   32.35  1976 -1907.4 -2000.1 -2004.1 inf     0.012225 989.38  
12 5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    5.684    0.3      1.456   32.35 1976 4.28   13.79  8.342  0.4074 1.468  0.9279 1.035  1.791  0.4792 1.44   3.224  1.914  7.249  0.6282 0.7326 7.659  3.34   0.5291 0.5596 0.5795 0.6521 0.4356 1.793  3.128  2.975  1.784  2.3    2.22   2.145  1.504  2.809  1.073  1.894  1.706  0.759  0.5404 1.028  0.8398 0.9142 0.5138 0.9806 21.42  6.47   0.3061 150.5  inf     -1405   1    0  1.4556   481.2    32.35  1976 1.4556   481.2    32.35  1976 -837.22 -916.78 -920.88 inf     0.0075928 603.52  
12 1.837    4.842    4.847    0.7693   1.262    1.106    1.587    1.504    0.7693   1.08     2.107    1.282    2.718    0.9815   0.79     3.426    1.506    0.8104   0.9759   0.7693   1.509    1.233    1.21     1.673    1.534    1.19     1.282    1.347    1.488    1.48     2.599    0.9447   1.653    1.321    1.493    1.066    1.003    0.9154   2.48     0.8512   1.778    4.585    3.903    0.7693   0.039935 0.9013  1130  1976 31.57  24.03  16.58  47.09  6.194  9.584  15.21  38.41  39.07  51.33  10.65  12.73  39.96  42.33  36.25  10.43  63.71  10.55  31.63  22.29  3.917  2.466  29.45  12.53  55.75  10.02  16.98  8.218  25.67  11     3.651  9.869  7.41   20.9   9.602  2.672  9.501  23.46  5.264  9.568  20.86  50.23  19.99  141.6  263    471.1   -685.9  1    0  0.90133  3946.8   1130   1976 0.90133  3946.8   1130   1976 3260.2  3167.1  3163.1  3731.4  0.00066838 2128.1  
12 1.217    2.885    2.554    0.9096   0.4139   0.5298   1.038    1.259    0.6736   1.04     0.9411   0.5647   2.068    1.115    0.6601   1.321    1.422    0.4185   1.027    0.5455   0.6408   0.5085   0.8578   0.7058   1.422    0.4653   0.6096   0.4702   1.002    0.778    0.8796   0.4291   0.6317   0.7991   0.9143   0.342    0.45     0.7114   1.644    0.4634   1.653    3.676    2.399    1.088    0.03244  0.6509  1237  1976 29.16  62.41  43.54  8.983  50.47  19.03  10.76  48.72  28.23  21.89  6.777  13.23  67.49  55.7   11.53  25.46  39.57  15.01  26.47  83.92  2.109  1.117  52.13  75.39  44.47  34.85  24.03  15.6   10.05  13.38  3.909  41.28  13.35  20.03  5.369  12.91  61.06  24.84  11.75  27.21  103.7  83.16  66.11  439.3  351.2  471.1   -419.7  1    0  0.65091  4288.7   1237   1976 0.65091  4288.7   1237   1976 3835.2  3735.7  3731.6  4306.3  0.00051646 2569.8  
12 0.7019   2.476    1.945    0.3233   0.3845   0.3203   0.4918   0.9819   0.4145   0.5339   0.2946   0.2256   1.78     1.146    0.2419   0.7485   0.9145   0.2154   0.6968   0.5965   0.1906   0.1387   0.6952   0.6758   0.9761   0.2996   0.3149   0.2038   0.3319   0.4007   0.3403   0.3245   0.2892   0.3963   0.3691   0.2366   0.4649   0.4363   1.405    0.3381   2.449    3.49     2.375    2.723    0.028306 0.591   1475  1976 25.88  91.27  64.09  7.548  41.83  15.31  24.34  27.01  11.21  27.64  17.69  5.548  45.48  28.64  18.15  34.28  87.71  21.1   31.09  31.1   1.127  0.4809 89.72  77.19  84.86  70.14  20.1   36.91  54.18  20.33  1.188  45.83  16.35  82.25  3.7    3.732  29.79  15.79  17.68  36.92  51.77  97.42  97.67  289.1  373.8  471.1   -175.5  1    0  0.59101  4447.4   1475   1976 0.59101  4447.4   1475   1976 4227.7  4127.1  4123    4698.8  0.00045068 2893.8  
12 0.375    2.503    1.753    0.108    0.2828   0.1681   0.3446   0.5517   0.1495   0.3168   0.168    0.0571   1.215    0.7462   0.1124   0.474    0.874    0.1326   0.4559   0.348    0.04988  0.03258  0.698    0.6229   0.9216   0.2652   0.1488   0.1358   0.2669   0.2503   0.07356  0.2373   0.1493   0.4171   0.1277   0.07676  0.2871   0.2122   1.258    0.2724   2.147    3.493    2.658    5.173    0.027162 0.5724  1552  1976 56.83  117.1  77.44  24.36  55.43  11.14  31.87  46.5   38.55  43.64  10.91  20.02  67.2   68.5   24.45  32.53  88.94  29.89  54.32  67.59  0.5338 0.4345 91.57  61.82  124.4  82.29  31.2   104.9  90.43  19.02  2.966  35.65  14.98  75.95  3.97   5.236  33.96  15.24  14.2   50.65  80.14  96.31  111.3  177.4  364.1  471.1   77.56   1    0  0.57236  4498.2   1552   1976 0.57236  4498.2   1552   1976 4501.2  4401.6  4397.6  4972.3  0.00042559 2933.1  
12 0.2992   2.806    1.696    0.07341  0.2355   0.08056  0.2753   0.4226   0.1086   0.244    0.07779  0.03182  1.008    0.75     0.06345  0.2909   0.8355   0.09739  0.3977   0.3037   0.009635 0.008693 0.6939   0.5028   1.048    0.2504   0.09081  0.154    0.2774   0.1541   0.02709  0.1537   0.07913  0.4048   0.05351  0.03141  0.1918   0.103    1.05     0.258    2.291    3.458    3.077    7.353    0.026649 0.5724  1612  1976 89.31  93.18  82.66  52.71  79.98  48.49  49.94  79.26  73.05  73.59  50.89  64.47  97.79  67.81  76.76  86.35  97.32  55.42  71.37  88.73  14.3   6.103  92.65  94.87  96.2   92.34  83.75  81.5   83.72  50.19  21.87  84.97  53.35  80.66  22.62  31.27  76.08  64.64  20.41  56.44  70.4   98.3   83.06  87.83  347.7  471.1   249.3   1    0  0.57236  4512.8   1612   1976 0.57236  4512.8   1612   1976 4636.8  4539.7  4535.6  5108    0.00041462 2931.2  
12 0.3022   2.779    1.693    0.07903  0.2376   0.09086  0.2822   0.4312   0.1129   0.2491   0.08794  0.03576  1.01     0.7407   0.06809  0.3059   0.8341   0.1018   0.3997   0.3047   0.01753  0.01145  0.6887   0.5056   1.04     0.2487   0.09629  0.1498   0.2721   0.1632   0.03274  0.1606   0.08898  0.3997   0.06551  0.03265  0.2019   0.1158   1.122    0.255    2.246    3.449    3.009    7.079    0.026514 0.5724  1628  1976 87.53  94.98  83.01  45.48  78.53  38.12  47.52  76.13  67.62  70.58  39.82  51.05  97.37  69.51  66.64  78.1   97.65  50.77  70.67  88.15  4.321  3.517  94.08  93.81  97.65  93.65  74.48  86.19  87.01  44.71  14.98  77.85  42.2   82.74  15.09  28.94  68.68  51.2   17.85  57.77  73.24  98.79  86.81  94.75  350.6  471.1   221.1   1    0  0.57236  4515.3   1628   1976 0.57236  4515.3   1628   1976 4618.6  4520.7  4516.7  5089.8  0.00041438 2958.5  
12 0.3021   2.781    1.693    0.07765  0.2378   0.08888  0.2812   0.4304   0.1123   0.2488   0.08591  0.03477  1.01     0.7427   0.06737  0.3039   0.8344   0.1009   0.4002   0.3049   0.01176  0.01061  0.6895   0.5058   1.041    0.249    0.09547  0.1504   0.273    0.1619   0.03098  0.1598   0.08675  0.4011   0.06177  0.03391  0.2003   0.1131   1.1      0.2561   2.254    3.45     3.02     7.1      0.026538 0.5724  1625  1976 87.55  94.88  82.95  47.11  78.44  39.84  47.86  76.42  68.35  70.77  41.73  54     97.34  69.14  68.09  79.13  97.58  51.59  70.49  88.05  9.597  4.095  93.84  93.77  97.56  93.36  75.76  85.52  86.43  45.45  16.72  78.62  44.39  82.16  16.98  26.83  69.8   53.69  18.59  57.27  72.68  98.71  86.22  94.2   349.9  471.1   230.1   1    0  0.57236  4514.9   1625   1976 0.57236  4514.9   1625   1976 4625.8  4528.2  4524.1  5096.9  0.00041437 2953.2  