Date and time of run 15-JAN-2007 11:07:27 > 20070115110339 MTDATA 4.74 2004-11-18 12:00, LOG D:\MTDATA\Work\mt48.log > 20070115110339 user2 on DVF-400-* using D:\MTDATA\DVF\mtdata.exe > 20070115110724 MODULE 3 creates MPI file D:\MTDATA\Work\def.mpi > 20070115110727 MODULE 3 reads MPI file D:\MTDATA\Work\def.mpi > 20070115110727 MODULE 3 creates MPR file D:\MTDATA\Work\def.mpr $(Number of lines of title) 8 * DATAFILE = D:\MTDATA\Work\def.mpi - CREATED 11:07:24 15-JAN-2007 * SYSTEM = C,Mn,Ni,Fe, * NUMBER OF PHASES = 23 * NUMBER OF SPECIES = 81 * DATA FILE = D:\MTDATA\Work\def.mpi *** PROBLEM settings *** SYSTEM ELEMENTS : CFeMnNi NUMBER COMPONENT STATUS AMOUNT DELTA REF.P 1 C NORMAL 10.9316 2 Mn #PARA! 41.4103 3 Ni #PARA! 68.7170 4 Fe # TO BAL 1675.30 NUMBER PHASE STATUS MODEL 1 DIAMOND_A4 absent PURE SUBSTANCE 2 GRAPHITE absent PURE SUBSTANCE 3 LIQUID absent REDLICH-KISTER 4 BCC_A2 NORMAL SUBLATTICE 5 CBCC_A12 absent SUBLATTICE 6 CEMENTITE absent SUBLATTICE 7 CUB_A13 absent SUBLATTICE 8 FCC_A1 1 M-G SUBLATTICE 9 FE4N absent SUBLATTICE 10 FECN_CHI absent PURE SUBSTANCE 11 HCP_A3 absent SUBLATTICE 12 KSI_CARBIDE absent PURE SUBSTANCE 13 M3C2 absent SUBLATTICE 14 M5C2 absent SUBLATTICE 15 M7C3 absent SUBLATTICE 16 V3C2 absent SUBLATTICE 17 M23C6 absent SUBLATTICE 18 AL5FE4 absent REDLICH-KISTER 19 ORTHORHOMBIC_A20 absent PURE SUBSTANCE 20 TETRAGONAL_U absent PURE SUBSTANCE 21 LAVES_C14 absent SUBLATTICE 22 LAVES_C15 absent SUBLATTICE 23 BCC_B2 absent CHEMICAL ORDERING(C) NUMBER SUBSTANCE STATUS/CONSTRAINT 1 C NORMAL 2 C NORMAL 3 C NORMAL 4 Fe NORMAL 5 Mn NORMAL 6 Ni NORMAL 7 Fe:1 NORMAL 8 Mn:1 NORMAL 9 Ni:1 NORMAL 10 C:2 NORMAL 11 Va:2 NORMAL 12 Fe:1 NORMAL 13 Mn:1 NORMAL 14 Ni:1 NORMAL 15 C:2 NORMAL 16 Va:2 NORMAL 17 Fe:1 NORMAL 18 Mn:1 NORMAL 19 Ni:1 NORMAL 20 C:2 NORMAL 21 Fe:1 NORMAL 22 Mn:1 NORMAL 23 Ni:1 NORMAL 24 C:2 NORMAL 25 Va:2 NORMAL 26 Fe:1 NORMAL 27 Mn:1 NORMAL 28 Ni:1 NORMAL 29 C:2 NORMAL 30 Va:2 NORMAL 31 Fe:1 NORMAL 32 Mn:1 NORMAL 33 Ni:1 NORMAL 34 C:2 NORMAL 35 Va:2 NORMAL 36 Fe5C2 NORMAL 37 Fe:1 NORMAL 38 Mn:1 NORMAL 39 Ni:1 NORMAL 40 C:2 NORMAL 41 Va:2 NORMAL 42 Fe3C NORMAL 43 Fe:1 NORMAL 44 Mn:1 NORMAL 45 C:2 NORMAL 46 Fe:1 NORMAL 47 Mn:1 NORMAL 48 C:2 NORMAL 49 Fe:1 NORMAL 50 Mn:1 NORMAL 51 Ni:1 NORMAL 52 C:2 NORMAL 53 Fe:1 NORMAL 54 Mn:1 NORMAL 55 C:2 NORMAL 56 Fe:1 NORMAL 57 Mn:1 NORMAL 58 Ni:1 NORMAL 59 Fe:2 NORMAL 60 Mn:2 NORMAL 61 Ni:2 NORMAL 62 C:3 NORMAL 63 Fe NORMAL 64 Mn NORMAL 65 Fe NORMAL 66 Fe NORMAL 67 Fe:1 NORMAL 68 Mn:1 NORMAL 69 Ni:1 NORMAL 70 Fe:2 NORMAL 71 Mn:2 NORMAL 72 Ni:2 NORMAL 73 Fe:1 NORMAL 74 Ni:1 NORMAL 75 Fe:2 NORMAL 76 Ni:2 NORMAL 77 Fe:1 NORMAL 78 Ni:1 NORMAL 79 Fe:2 NORMAL 80 Ni:2 NORMAL 81 Va:3 NORMAL UNARY SOURCE Tmin/K Tmax/K C mtsol 298.15 6000.00 C mtsol 298.15 6000.00 C mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Mn mtsol 298.15 2000.00 Ni mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C NODATA 298.15 298.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe5C2 mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe3C mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 6000.00 Fe:Fe:C mtsol 298.15 6000.00 Fe:Mn:C mtsol 298.15 2000.00 Fe:Ni:C mtsol 298.15 3000.00 Mn:Fe:C mtsol 298.15 2000.00 Mn:Mn:C mtsol 298.15 2000.00 Mn:Ni:C NODATA 298.15 298.00 Ni:Fe:C mtsol 298.15 3000.00 Ni:Mn:C NODATA 298.15 298.00 Ni:Ni:C mtsol 298.15 3000.00 Fe mtsol 298.15 6000.00 Mn mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Fe:Fe mtsol 298.15 6000.00 Fe:Mn NODATA 298.15 298.00 Fe:Ni NODATA 298.15 298.00 Mn:Fe NODATA 298.15 298.00 Mn:Mn mtsol 298.15 2000.00 Mn:Ni NODATA 298.15 298.00 Ni:Fe NODATA 298.15 298.00 Ni:Mn NODATA 298.15 298.00 Ni:Ni mtsol 298.15 3000.00 Fe:Fe mtsol 298.15 6000.00 Fe:Ni NODATA 298.15 298.00 Ni:Fe NODATA 298.15 298.00 Ni:Ni mtsol 298.15 3000.00 Fe:Fe:Va mtsol 298.15 6000.00 Fe:Ni:Va NODATA 298.15 298.00 Ni:Fe:Va NODATA 298.15 298.00 Ni:Ni:Va mtsol 298.15 3000.00 TEMPERATURE : 993.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 Stage 1* only requested *** MULTIPHASE - Stage 1* Results *** Temperature = 993.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7964E+03 FCC_A1 0.0060854 0.0230523 0.0382534 Fe 1.7964E+03 FCC_A1 0.9326089 Gibbs Energy = -7.9269959518E+07 J System Enthalpy = 4.9920639312E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 973.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 973.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 3.6552E+02 BCC_A2 0.0001313 0.0082764 0.0137340 1.4308E+03 FCC_A1 0.0076065 0.0268270 0.0445172 Fe 3.6552E+02 BCC_A2 0.9778584 1.4308E+03 FCC_A1 0.9210494 Gibbs Energy = -7.6692545581E+07 J System Enthalpy = 4.7424851456E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 953.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 953.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 6.6456E+02 BCC_A2 0.0001458 0.0087767 0.0145642 1.1318E+03 FCC_A1 0.0095730 0.0314346 0.0521630 Fe 6.6456E+02 BCC_A2 0.9765133 1.1318E+03 FCC_A1 0.9068294 Gibbs Energy = -7.4167682641E+07 J System Enthalpy = 4.4941817338E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 933.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 933.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 8.8485E+02 BCC_A2 0.0001591 0.0091874 0.0152458 9.1152E+02 FCC_A1 0.0118384 0.0365115 0.0605878 Fe 8.8485E+02 BCC_A2 0.9754077 9.1152E+02 FCC_A1 0.8910624 Gibbs Energy = -7.1693203611E+07 J System Enthalpy = 4.2620091430E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 913.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 913.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.0492E+03 BCC_A2 0.0001706 0.0094971 0.0157597 7.4712E+02 FCC_A1 0.0143922 0.0420891 0.0698434 Fe 1.0492E+03 BCC_A2 0.9745726 7.4712E+02 FCC_A1 0.8736753 Gibbs Energy = -6.9266877448E+07 J System Enthalpy = 4.0444594186E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 893.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 893.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.1737E+03 BCC_A2 0.0001800 0.0096991 0.0160948 6.2269E+02 FCC_A1 0.0172162 0.0482209 0.0800186 Fe 1.1737E+03 BCC_A2 0.9740262 6.2269E+02 FCC_A1 0.8545443 Gibbs Energy = -6.6886772130E+07 J System Enthalpy = 3.8395466528E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 873.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 873.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.2692E+03 BCC_A2 0.0001870 0.0097897 0.0162452 5.2715E+02 FCC_A1 0.0202870 0.0549846 0.0912424 Fe 1.2692E+03 BCC_A2 0.9737780 5.2715E+02 FCC_A1 0.8334860 Gibbs Energy = -6.4551317410E+07 J System Enthalpy = 3.6453019138E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 853.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 853.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.3437E+03 BCC_A2 0.0001917 0.0097680 0.0162091 4.5267E+02 FCC_A1 0.0235801 0.0624847 0.1036882 Fe 1.3437E+03 BCC_A2 0.9738313 4.5267E+02 FCC_A1 0.8102469 Gibbs Energy = -6.2259301174E+07 J System Enthalpy = 3.4599535846E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 833.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 833.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.4026E+03 BCC_A2 0.0001940 0.0096345 0.0159876 3.9372E+02 FCC_A1 0.0270740 0.0708544 0.1175770 Fe 1.4026E+03 BCC_A2 0.9741839 3.9372E+02 FCC_A1 0.7844946 Gibbs Energy = -6.0009841373E+07 J System Enthalpy = 3.2819735890E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 813.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 813.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.4501E+03 BCC_A2 0.0001944 0.0093920 0.0155853 3.4629E+02 FCC_A1 0.0307539 0.0802540 0.1331748 Fe 1.4501E+03 BCC_A2 0.9748283 3.4629E+02 FCC_A1 0.7558173 Gibbs Energy = -5.7802350502E+07 J System Enthalpy = 3.1100799341E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 793.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 793.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.4889E+03 BCC_A2 0.0001930 0.0090460 0.0150112 3.0751E+02 FCC_A1 0.0346144 0.0908656 0.1507839 Fe 1.4889E+03 BCC_A2 0.9757498 3.0751E+02 FCC_A1 0.7237361 Gibbs Energy = -5.5636498928E+07 J System Enthalpy = 2.9432206610E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 773.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 773.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5211E+03 BCC_A2 0.0001902 0.0086055 0.0142801 2.7530E+02 FCC_A1 0.0386574 0.1028725 0.1707084 Fe 1.5211E+03 BCC_A2 0.9769242 2.7530E+02 FCC_A1 0.6877618 Gibbs Energy = -5.3512175942E+07 J System Enthalpy = 2.7805798278E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 753.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 753.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5482E+03 BCC_A2 0.0001858 0.0080842 0.0134150 2.4820E+02 FCC_A1 0.0428843 0.1164159 0.1931826 Fe 1.5482E+03 BCC_A2 0.9783151 2.4820E+02 FCC_A1 0.6475172 Gibbs Energy = -5.1429443556E+07 J System Enthalpy = 2.6215968063E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 733.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 733.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5711E+03 BCC_A2 0.0001793 0.0075013 0.0124479 2.2525E+02 FCC_A1 0.0472811 0.1315222 0.2182503 Fe 1.5711E+03 BCC_A2 0.9798715 2.2525E+02 FCC_A1 0.6029464 Gibbs Energy = -4.9388478385E+07 J System Enthalpy = 2.4659960180E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 713.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 713.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5905E+03 BCC_A2 0.0001696 0.0068811 0.0114187 2.0583E+02 FCC_A1 0.0517994 0.1480144 0.2456176 Fe 1.5905E+03 BCC_A2 0.9815306 2.0583E+02 FCC_A1 0.5545686 Gibbs Energy = -4.7389501539E+07 J System Enthalpy = 2.3137906971E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 693.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 693.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6068E+03 BCC_A2 0.0001552 0.0062492 0.0103700 1.8958E+02 FCC_A1 0.0563465 0.1654664 0.2745778 Fe 1.6068E+03 BCC_A2 0.9832256 1.8958E+02 FCC_A1 0.5036093 Gibbs Energy = -4.5432709355E+07 J System Enthalpy = 2.1652105610E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 673.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 673.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6202E+03 BCC_A2 0.0001353 0.0056281 0.0093394 1.7620E+02 FCC_A1 0.0607969 0.1832679 0.3041178 Fe 1.6202E+03 BCC_A2 0.9848972 1.7620E+02 FCC_A1 0.4518174 Gibbs Energy = -4.3518230003E+07 J System Enthalpy = 2.0205466110E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 653.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 653.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6310E+03 BCC_A2 0.0001107 0.0050337 0.0083530 1.6535E+02 FCC_A1 0.0650189 0.2007844 0.3331851 Fe 1.6310E+03 BCC_A2 0.9865027 1.6535E+02 FCC_A1 0.4010115 Gibbs Energy = -4.1646124059E+07 J System Enthalpy = 1.8799947870E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 633.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 633.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6397E+03 BCC_A2 0.0000841 0.0044742 0.0074246 1.5666E+02 FCC_A1 0.0688989 0.2175026 0.3609275 Fe 1.6397E+03 BCC_A2 0.9880171 1.5666E+02 FCC_A1 0.3526709 Gibbs Energy = -3.9816420241E+07 J System Enthalpy = 1.7435912548E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 613.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 613.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6466E+03 BCC_A2 0.0000590 0.0039524 0.0065586 1.4974E+02 FCC_A1 0.0723539 0.2330815 0.3867794 Fe 1.6466E+03 BCC_A2 0.9894300 1.4974E+02 FCC_A1 0.3077852 Gibbs Energy = -3.8029160560E+07 J System Enthalpy = 1.6112365833E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 593.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 593.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6521E+03 BCC_A2 0.0000382 0.0034675 0.0057541 1.4426E+02 FCC_A1 0.0753384 0.2473360 0.4104336 Fe 1.6521E+03 BCC_A2 0.9907403 1.4426E+02 FCC_A1 0.2668920 Gibbs Energy = -3.6284437748E+07 J System Enthalpy = 1.4827446894E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 573.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.93165 41.41032 68.71699 1675.304 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1313000 2.275000 4.033000 93.56070 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 573.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.093165E+01 1.313000E-01 Mn undef undef 4.141032E+01 2.275000E+00 Ni undef undef 6.871699E+01 4.033000E+00 Fe undef undef 1.675304E+03 9.356070E+01 Total 1.796363E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6564E+03 BCC_A2 0.0000228 0.0030176 0.0050075 1.3994E+02 FCC_A1 0.0778492 0.2602025 0.4317845 Fe 1.6564E+03 BCC_A2 0.9919521 1.3994E+02 FCC_A1 0.2301638 Gibbs Energy = -3.4582422715E+07 J System Enthalpy = 1.3578810946E+07 J