Date and time of run 15-JAN-2007 21:45:03 > 20070115213804 MTDATA 4.74 2004-11-18 12:00, LOG D:\MTDATA\Work\mt51.log > 20070115213804 user2 on DVF-400-* using D:\MTDATA\DVF\mtdata.exe > 20070115214503 MODULE 3 creates MPI file D:\MTDATA\Work\def.mpi > 20070115214503 MODULE 3 reads MPI file D:\MTDATA\Work\def.mpi > 20070115214503 MODULE 3 creates MPR file D:\MTDATA\Work\def.mpr $(Number of lines of title) 8 * DATAFILE = D:\MTDATA\Work\def.mpi - CREATED 21:45:03 15-JAN-2007 * SYSTEM = C,Mn,Ni,Fe, * NUMBER OF PHASES = 23 * NUMBER OF SPECIES = 81 * DATA FILE = D:\MTDATA\Work\def.mpi *** PROBLEM settings *** SYSTEM ELEMENTS : CFeMnNi NUMBER COMPONENT STATUS AMOUNT DELTA REF.P 1 C NORMAL 10.4321 2 Mn #PARA! 41.2647 3 Ni #PARA! 85.5342 4 Fe #PARA! 1657.88 NUMBER PHASE STATUS MODEL 1 DIAMOND_A4 absent PURE SUBSTANCE 2 GRAPHITE absent PURE SUBSTANCE 3 LIQUID absent REDLICH-KISTER 4 BCC_A2 NORMAL SUBLATTICE 5 CBCC_A12 absent SUBLATTICE 6 CEMENTITE absent SUBLATTICE 7 CUB_A13 absent SUBLATTICE 8 FCC_A1 1 M-G SUBLATTICE 9 FE4N absent SUBLATTICE 10 FECN_CHI absent PURE SUBSTANCE 11 HCP_A3 absent SUBLATTICE 12 KSI_CARBIDE absent PURE SUBSTANCE 13 M3C2 absent SUBLATTICE 14 M5C2 absent SUBLATTICE 15 M7C3 absent SUBLATTICE 16 V3C2 absent SUBLATTICE 17 M23C6 absent SUBLATTICE 18 AL5FE4 absent REDLICH-KISTER 19 ORTHORHOMBIC_A20 absent PURE SUBSTANCE 20 TETRAGONAL_U absent PURE SUBSTANCE 21 LAVES_C14 absent SUBLATTICE 22 LAVES_C15 absent SUBLATTICE 23 BCC_B2 absent CHEMICAL ORDERING(C) NUMBER SUBSTANCE STATUS/CONSTRAINT 1 C NORMAL 2 C NORMAL 3 C NORMAL 4 Fe NORMAL 5 Mn NORMAL 6 Ni NORMAL 7 Fe:1 NORMAL 8 Mn:1 NORMAL 9 Ni:1 NORMAL 10 C:2 NORMAL 11 Va:2 NORMAL 12 Fe:1 NORMAL 13 Mn:1 NORMAL 14 Ni:1 NORMAL 15 C:2 NORMAL 16 Va:2 NORMAL 17 Fe:1 NORMAL 18 Mn:1 NORMAL 19 Ni:1 NORMAL 20 C:2 NORMAL 21 Fe:1 NORMAL 22 Mn:1 NORMAL 23 Ni:1 NORMAL 24 C:2 NORMAL 25 Va:2 NORMAL 26 Fe:1 NORMAL 27 Mn:1 NORMAL 28 Ni:1 NORMAL 29 C:2 NORMAL 30 Va:2 NORMAL 31 Fe:1 NORMAL 32 Mn:1 NORMAL 33 Ni:1 NORMAL 34 C:2 NORMAL 35 Va:2 NORMAL 36 Fe5C2 NORMAL 37 Fe:1 NORMAL 38 Mn:1 NORMAL 39 Ni:1 NORMAL 40 C:2 NORMAL 41 Va:2 NORMAL 42 Fe3C NORMAL 43 Fe:1 NORMAL 44 Mn:1 NORMAL 45 C:2 NORMAL 46 Fe:1 NORMAL 47 Mn:1 NORMAL 48 C:2 NORMAL 49 Fe:1 NORMAL 50 Mn:1 NORMAL 51 Ni:1 NORMAL 52 C:2 NORMAL 53 Fe:1 NORMAL 54 Mn:1 NORMAL 55 C:2 NORMAL 56 Fe:1 NORMAL 57 Mn:1 NORMAL 58 Ni:1 NORMAL 59 Fe:2 NORMAL 60 Mn:2 NORMAL 61 Ni:2 NORMAL 62 C:3 NORMAL 63 Fe NORMAL 64 Mn NORMAL 65 Fe NORMAL 66 Fe NORMAL 67 Fe:1 NORMAL 68 Mn:1 NORMAL 69 Ni:1 NORMAL 70 Fe:2 NORMAL 71 Mn:2 NORMAL 72 Ni:2 NORMAL 73 Fe:1 NORMAL 74 Ni:1 NORMAL 75 Fe:2 NORMAL 76 Ni:2 NORMAL 77 Fe:1 NORMAL 78 Ni:1 NORMAL 79 Fe:2 NORMAL 80 Ni:2 NORMAL 81 Va:3 NORMAL UNARY SOURCE Tmin/K Tmax/K C mtsol 298.15 6000.00 C mtsol 298.15 6000.00 C mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Mn mtsol 298.15 2000.00 Ni mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C NODATA 298.15 298.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe5C2 mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe3C mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 6000.00 Fe:Fe:C mtsol 298.15 6000.00 Fe:Mn:C mtsol 298.15 2000.00 Fe:Ni:C mtsol 298.15 3000.00 Mn:Fe:C mtsol 298.15 2000.00 Mn:Mn:C mtsol 298.15 2000.00 Mn:Ni:C NODATA 298.15 298.00 Ni:Fe:C mtsol 298.15 3000.00 Ni:Mn:C NODATA 298.15 298.00 Ni:Ni:C mtsol 298.15 3000.00 Fe mtsol 298.15 6000.00 Mn mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Fe:Fe mtsol 298.15 6000.00 Fe:Mn NODATA 298.15 298.00 Fe:Ni NODATA 298.15 298.00 Mn:Fe NODATA 298.15 298.00 Mn:Mn mtsol 298.15 2000.00 Mn:Ni NODATA 298.15 298.00 Ni:Fe NODATA 298.15 298.00 Ni:Mn NODATA 298.15 298.00 Ni:Ni mtsol 298.15 3000.00 Fe:Fe mtsol 298.15 6000.00 Fe:Ni NODATA 298.15 298.00 Ni:Fe NODATA 298.15 298.00 Ni:Ni mtsol 298.15 3000.00 Fe:Fe:Va mtsol 298.15 6000.00 Fe:Ni:Va NODATA 298.15 298.00 Ni:Fe:Va NODATA 298.15 298.00 Ni:Ni:Va mtsol 298.15 3000.00 TEMPERATURE : 993.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 Stage 1* only requested *** MULTIPHASE - Stage 1* Results *** Temperature = 993.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7951E+03 FCC_A1 0.0058114 0.0229873 0.0476484 Fe 1.7951E+03 FCC_A1 0.9235530 Gibbs Energy = -7.9766105259E+07 J System Enthalpy = 4.9690200561E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 973.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 973.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7951E+03 FCC_A1 0.0058114 0.0229873 0.0476484 Fe 1.7951E+03 FCC_A1 0.9235530 Gibbs Energy = -7.7170862891E+07 J System Enthalpy = 4.8532969450E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 953.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 953.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7951E+03 FCC_A1 0.0058114 0.0229873 0.0476484 Fe 1.7951E+03 FCC_A1 0.9235530 Gibbs Energy = -7.4599340966E+07 J System Enthalpy = 4.7381966572E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 933.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 933.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7951E+03 FCC_A1 0.0058114 0.0229873 0.0476484 Fe 1.7951E+03 FCC_A1 0.9235530 Gibbs Energy = -7.2051906508E+07 J System Enthalpy = 4.6237198564E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 913.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 913.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7951E+03 FCC_A1 0.0058114 0.0229873 0.0476484 Fe 1.7951E+03 FCC_A1 0.9235530 Gibbs Energy = -6.9528942123E+07 J System Enthalpy = 4.5098673419E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 893.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 893.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 7.8086E+02 BCC_A2 0.0000912 0.0231195 0.0479225 1.0143E+03 FCC_A1 0.0102153 0.0228854 0.0474373 Fe 7.8086E+02 BCC_A2 0.9288668 1.0143E+03 FCC_A1 0.9194620 Gibbs Energy = -6.7047453175E+07 J System Enthalpy = 4.1099309201E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 873.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 873.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.2886E+03 BCC_A2 0.0001664 0.0231178 0.0479189 5.0654E+02 FCC_A1 0.0201714 0.0226552 0.0469601 Fe 1.2886E+03 BCC_A2 0.9287969 5.0654E+02 FCC_A1 0.9102132 Gibbs Energy = -6.4668148673E+07 J System Enthalpy = 3.7725263818E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 853.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 853.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.4601E+03 BCC_A2 0.0002295 0.0231163 0.0479159 3.3498E+02 FCC_A1 0.0301426 0.0224247 0.0464822 Fe 1.4601E+03 BCC_A2 0.9287383 3.3498E+02 FCC_A1 0.9009505 Gibbs Energy = -6.2349087548E+07 J System Enthalpy = 3.5530497097E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 833.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 833.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5454E+03 BCC_A2 0.0002804 0.0231151 0.0479134 2.4970E+02 FCC_A1 0.0400430 0.0221958 0.0460077 Fe 1.5454E+03 BCC_A2 0.9286910 2.4970E+02 FCC_A1 0.8917535 Gibbs Energy = -6.0076862499E+07 J System Enthalpy = 3.3676995809E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 813.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 813.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5959E+03 BCC_A2 0.0003197 0.0231142 0.0479116 1.9917E+02 FCC_A1 0.0498155 0.0219698 0.0455394 Fe 1.5959E+03 BCC_A2 0.9286545 1.9917E+02 FCC_A1 0.8826753 Gibbs Energy = -5.7846960378E+07 J System Enthalpy = 3.1987861056E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 793.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 793.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6291E+03 BCC_A2 0.0003477 0.0231136 0.0479102 1.6603E+02 FCC_A1 0.0594226 0.0217477 0.0450789 Fe 1.6291E+03 BCC_A2 0.9286285 1.6603E+02 FCC_A1 0.8737508 Gibbs Energy = -5.5657261521E+07 J System Enthalpy = 3.0400804589E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 773.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 773.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6523E+03 BCC_A2 0.0003652 0.0231132 0.0479094 1.4277E+02 FCC_A1 0.0688407 0.0215299 0.0446276 Fe 1.6523E+03 BCC_A2 0.9286123 1.4277E+02 FCC_A1 0.8650018 Gibbs Energy = -5.3506609755E+07 J System Enthalpy = 2.8887186617E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 753.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 753.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6694E+03 BCC_A2 0.0003730 0.0231130 0.0479090 1.2567E+02 FCC_A1 0.0780554 0.0213169 0.0441859 Fe 1.6694E+03 BCC_A2 0.9286050 1.2567E+02 FCC_A1 0.8564418 Gibbs Energy = -5.1394337101E+07 J System Enthalpy = 2.7431377186E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 733.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 733.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6825E+03 BCC_A2 0.0003720 0.0231130 0.0479091 1.1264E+02 FCC_A1 0.0870593 0.0211087 0.0437544 Fe 1.6825E+03 BCC_A2 0.9286059 1.1264E+02 FCC_A1 0.8480777 Gibbs Energy = -4.9320065609E+07 J System Enthalpy = 2.6023754145E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 713.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 713.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.6927E+03 BCC_A2 0.0003634 0.0231132 0.0479095 1.0242E+02 FCC_A1 0.0958490 0.0209054 0.0433331 Fe 1.6927E+03 BCC_A2 0.9286139 1.0242E+02 FCC_A1 0.8399124 Gibbs Energy = -4.7283611700E+07 J System Enthalpy = 2.4657847126E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 693.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 693.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7009E+03 BCC_A2 0.0003482 0.0231136 0.0479102 9.4229E+01 FCC_A1 0.1044246 0.0207072 0.0429221 Fe 1.7009E+03 BCC_A2 0.9286280 9.4229E+01 FCC_A1 0.8319461 Gibbs Energy = -4.5284935108E+07 J System Enthalpy = 2.3329006279E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 673.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 673.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7076E+03 BCC_A2 0.0003276 0.0231140 0.0479112 8.7533E+01 FCC_A1 0.1127883 0.0205138 0.0425213 Fe 1.7076E+03 BCC_A2 0.9286472 8.7533E+01 FCC_A1 0.8241766 Gibbs Energy = -4.3324109747E+07 J System Enthalpy = 2.2033715958E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 653.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 653.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7131E+03 BCC_A2 0.0003027 0.0231146 0.0479124 8.1968E+01 FCC_A1 0.1209435 0.0203252 0.0421304 Fe 1.7131E+03 BCC_A2 0.9286703 8.1968E+01 FCC_A1 0.8166008 Gibbs Energy = -4.1401306449E+07 J System Enthalpy = 2.0769211050E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 633.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 633.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7178E+03 BCC_A2 0.0002748 0.0231153 0.0479137 7.7273E+01 FCC_A1 0.1288949 0.0201414 0.0417494 Fe 1.7178E+03 BCC_A2 0.9286962 7.7273E+01 FCC_A1 0.8092144 Gibbs Energy = -3.9516782695E+07 J System Enthalpy = 1.9533248070E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 613.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 613.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7219E+03 BCC_A2 0.0002450 0.0231160 0.0479151 7.3256E+01 FCC_A1 0.1366473 0.0199621 0.0413778 Fe 1.7219E+03 BCC_A2 0.9287239 7.3256E+01 FCC_A1 0.8020127 Gibbs Energy = -3.7670876817E+07 J System Enthalpy = 1.8323961115E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 593.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 593.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7253E+03 BCC_A2 0.0002143 0.0231167 0.0479166 6.9777E+01 FCC_A1 0.1442064 0.0197873 0.0410155 Fe 1.7253E+03 BCC_A2 0.9287524 6.9777E+01 FCC_A1 0.7949907 Gibbs Energy = -3.5864005247E+07 J System Enthalpy = 1.7139767096E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 573.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 10.43210 41.26470 85.53416 1657.881 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.1253000 2.267000 5.020000 92.58770 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 573.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.043210E+01 1.253000E-01 Mn undef undef 4.126470E+01 2.267000E+00 Ni undef undef 8.553416E+01 5.020000E+00 Fe undef undef 1.657881E+03 9.258770E+01 Total 1.795112E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7284E+03 BCC_A2 0.0001839 0.0231174 0.0479181 6.6727E+01 FCC_A1 0.1515778 0.0196169 0.0406622 Fe 1.7284E+03 BCC_A2 0.9287807 6.6727E+01 FCC_A1 0.7881431 Gibbs Energy = -3.4096662054E+07 J System Enthalpy = 1.5979301299E+07 J