Date and time of run 15-JAN-2007 11:13:40 > 20070115110339 MTDATA 4.74 2004-11-18 12:00, LOG D:\MTDATA\Work\mt48.log > 20070115110339 user2 on DVF-400-* using D:\MTDATA\DVF\mtdata.exe > 20070115111337 MODULE 3 creates MPI file D:\MTDATA\Work\def.mpi > 20070115111340 MODULE 3 reads MPI file D:\MTDATA\Work\def.mpi > 20070115111340 MODULE 3 creates MPR file D:\MTDATA\Work\def.mpr $(Number of lines of title) 8 * DATAFILE = D:\MTDATA\Work\def.mpi - CREATED 11:13:37 15-JAN-2007 * SYSTEM = C,Mn,Ni,Fe, * NUMBER OF PHASES = 23 * NUMBER OF SPECIES = 81 * DATA FILE = D:\MTDATA\Work\def.mpi *** PROBLEM settings *** SYSTEM ELEMENTS : CFeMnNi NUMBER COMPONENT STATUS AMOUNT DELTA REF.P 1 C NORMAL 16.8179 2 Mn #PARA! 45.5787 3 Ni #PARA! 114.807 4 Fe # TO BAL 1621.50 NUMBER PHASE STATUS MODEL 1 DIAMOND_A4 absent PURE SUBSTANCE 2 GRAPHITE absent PURE SUBSTANCE 3 LIQUID absent REDLICH-KISTER 4 BCC_A2 NORMAL SUBLATTICE 5 CBCC_A12 absent SUBLATTICE 6 CEMENTITE absent SUBLATTICE 7 CUB_A13 absent SUBLATTICE 8 FCC_A1 1 M-G SUBLATTICE 9 FE4N absent SUBLATTICE 10 FECN_CHI absent PURE SUBSTANCE 11 HCP_A3 absent SUBLATTICE 12 KSI_CARBIDE absent PURE SUBSTANCE 13 M3C2 absent SUBLATTICE 14 M5C2 absent SUBLATTICE 15 M7C3 absent SUBLATTICE 16 V3C2 absent SUBLATTICE 17 M23C6 absent SUBLATTICE 18 AL5FE4 absent REDLICH-KISTER 19 ORTHORHOMBIC_A20 absent PURE SUBSTANCE 20 TETRAGONAL_U absent PURE SUBSTANCE 21 LAVES_C14 absent SUBLATTICE 22 LAVES_C15 absent SUBLATTICE 23 BCC_B2 absent CHEMICAL ORDERING(C) NUMBER SUBSTANCE STATUS/CONSTRAINT 1 C NORMAL 2 C NORMAL 3 C NORMAL 4 Fe NORMAL 5 Mn NORMAL 6 Ni NORMAL 7 Fe:1 NORMAL 8 Mn:1 NORMAL 9 Ni:1 NORMAL 10 C:2 NORMAL 11 Va:2 NORMAL 12 Fe:1 NORMAL 13 Mn:1 NORMAL 14 Ni:1 NORMAL 15 C:2 NORMAL 16 Va:2 NORMAL 17 Fe:1 NORMAL 18 Mn:1 NORMAL 19 Ni:1 NORMAL 20 C:2 NORMAL 21 Fe:1 NORMAL 22 Mn:1 NORMAL 23 Ni:1 NORMAL 24 C:2 NORMAL 25 Va:2 NORMAL 26 Fe:1 NORMAL 27 Mn:1 NORMAL 28 Ni:1 NORMAL 29 C:2 NORMAL 30 Va:2 NORMAL 31 Fe:1 NORMAL 32 Mn:1 NORMAL 33 Ni:1 NORMAL 34 C:2 NORMAL 35 Va:2 NORMAL 36 Fe5C2 NORMAL 37 Fe:1 NORMAL 38 Mn:1 NORMAL 39 Ni:1 NORMAL 40 C:2 NORMAL 41 Va:2 NORMAL 42 Fe3C NORMAL 43 Fe:1 NORMAL 44 Mn:1 NORMAL 45 C:2 NORMAL 46 Fe:1 NORMAL 47 Mn:1 NORMAL 48 C:2 NORMAL 49 Fe:1 NORMAL 50 Mn:1 NORMAL 51 Ni:1 NORMAL 52 C:2 NORMAL 53 Fe:1 NORMAL 54 Mn:1 NORMAL 55 C:2 NORMAL 56 Fe:1 NORMAL 57 Mn:1 NORMAL 58 Ni:1 NORMAL 59 Fe:2 NORMAL 60 Mn:2 NORMAL 61 Ni:2 NORMAL 62 C:3 NORMAL 63 Fe NORMAL 64 Mn NORMAL 65 Fe NORMAL 66 Fe NORMAL 67 Fe:1 NORMAL 68 Mn:1 NORMAL 69 Ni:1 NORMAL 70 Fe:2 NORMAL 71 Mn:2 NORMAL 72 Ni:2 NORMAL 73 Fe:1 NORMAL 74 Ni:1 NORMAL 75 Fe:2 NORMAL 76 Ni:2 NORMAL 77 Fe:1 NORMAL 78 Ni:1 NORMAL 79 Fe:2 NORMAL 80 Ni:2 NORMAL 81 Va:3 NORMAL UNARY SOURCE Tmin/K Tmax/K C mtsol 298.15 6000.00 C mtsol 298.15 6000.00 C mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Mn mtsol 298.15 2000.00 Ni mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C NODATA 298.15 298.00 Mn:Va mtsol 298.15 2000.00 Ni:C NODATA 298.15 298.00 Ni:Va mtsol 298.15 3000.00 Fe5C2 mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Fe:Va mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Mn:Va mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Ni:Va mtsol 298.15 3000.00 Fe3C mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 6000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 2000.00 Ni:C mtsol 298.15 3000.00 Fe:C mtsol 298.15 6000.00 Mn:C mtsol 298.15 6000.00 Fe:Fe:C mtsol 298.15 6000.00 Fe:Mn:C mtsol 298.15 2000.00 Fe:Ni:C mtsol 298.15 3000.00 Mn:Fe:C mtsol 298.15 2000.00 Mn:Mn:C mtsol 298.15 2000.00 Mn:Ni:C NODATA 298.15 298.00 Ni:Fe:C mtsol 298.15 3000.00 Ni:Mn:C NODATA 298.15 298.00 Ni:Ni:C mtsol 298.15 3000.00 Fe mtsol 298.15 6000.00 Mn mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Fe mtsol 298.15 6000.00 Fe:Fe mtsol 298.15 6000.00 Fe:Mn NODATA 298.15 298.00 Fe:Ni NODATA 298.15 298.00 Mn:Fe NODATA 298.15 298.00 Mn:Mn mtsol 298.15 2000.00 Mn:Ni NODATA 298.15 298.00 Ni:Fe NODATA 298.15 298.00 Ni:Mn NODATA 298.15 298.00 Ni:Ni mtsol 298.15 3000.00 Fe:Fe mtsol 298.15 6000.00 Fe:Ni NODATA 298.15 298.00 Ni:Fe NODATA 298.15 298.00 Ni:Ni mtsol 298.15 3000.00 Fe:Fe:Va mtsol 298.15 6000.00 Fe:Ni:Va NODATA 298.15 298.00 Ni:Fe:Va NODATA 298.15 298.00 Ni:Ni:Va mtsol 298.15 3000.00 TEMPERATURE : 993.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 Stage 1* only requested *** MULTIPHASE - Stage 1* Results *** Temperature = 993.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7987E+03 FCC_A1 0.0093500 0.0253397 0.0638274 Fe 1.7987E+03 FCC_A1 0.9014829 Gibbs Energy = -8.0871235122E+07 J System Enthalpy = 4.9580295562E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 973.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 973.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7987E+03 FCC_A1 0.0093500 0.0253397 0.0638274 Fe 1.7987E+03 FCC_A1 0.9014829 Gibbs Energy = -7.8255960346E+07 J System Enthalpy = 4.8422144410E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 953.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 953.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.7987E+03 FCC_A1 0.0093500 0.0253397 0.0638274 Fe 1.7987E+03 FCC_A1 0.9014829 Gibbs Energy = -7.5664424619E+07 J System Enthalpy = 4.7270250990E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 933.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 933.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 2.3982E+02 BCC_A2 0.0001542 0.0073347 0.0184751 1.5589E+03 FCC_A1 0.0107647 0.0281096 0.0708045 Fe 2.3982E+02 BCC_A2 0.9740361 1.5589E+03 FCC_A1 0.8903212 Gibbs Energy = -7.3104885207E+07 J System Enthalpy = 4.5075185280E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 913.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 913.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 5.1171E+02 BCC_A2 0.0001665 0.0076312 0.0192219 1.2870E+03 FCC_A1 0.0130014 0.0323807 0.0815627 Fe 5.1171E+02 BCC_A2 0.9729805 1.2870E+03 FCC_A1 0.8730551 Gibbs Energy = -7.0599106705E+07 J System Enthalpy = 4.2590115004E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 893.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 893.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 7.2029E+02 BCC_A2 0.0001774 0.0078422 0.0197533 1.0784E+03 FCC_A1 0.0154766 0.0370267 0.0932654 Fe 7.2029E+02 BCC_A2 0.9722271 1.0784E+03 FCC_A1 0.8542313 Gibbs Energy = -6.8145842081E+07 J System Enthalpy = 4.0274780916E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 873.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 873.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 8.8249E+02 BCC_A2 0.0001870 0.0079639 0.0200599 9.1621E+02 FCC_A1 0.0181758 0.0420761 0.1059841 Fe 8.8249E+02 BCC_A2 0.9717892 9.1621E+02 FCC_A1 0.8337640 Gibbs Energy = -6.5742750829E+07 J System Enthalpy = 3.8104131247E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 853.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 853.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.0103E+03 BCC_A2 0.0001951 0.0079950 0.0201382 7.8841E+02 FCC_A1 0.0210815 0.0475660 0.1198124 Fe 1.0103E+03 BCC_A2 0.9716717 7.8841E+02 FCC_A1 0.8115402 Gibbs Energy = -6.3387937173E+07 J System Enthalpy = 3.6055300465E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 833.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 833.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.1123E+03 BCC_A2 0.0002017 0.0079362 0.0199902 6.8642E+02 FCC_A1 0.0241741 0.0535406 0.1348618 Fe 1.1123E+03 BCC_A2 0.9718720 6.8642E+02 FCC_A1 0.7874235 Gibbs Energy = -6.1079916309E+07 J System Enthalpy = 3.4108561952E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 813.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 813.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.1947E+03 BCC_A2 0.0002069 0.0077905 0.0196231 6.0404E+02 FCC_A1 0.0274332 0.0600485 0.1512543 Fe 1.1947E+03 BCC_A2 0.9723795 6.0404E+02 FCC_A1 0.7612640 Gibbs Energy = -5.8817565888E+07 J System Enthalpy = 3.2247475178E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 793.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 793.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.2620E+03 BCC_A2 0.0002108 0.0075629 0.0190500 5.3674E+02 FCC_A1 0.0308382 0.0671364 0.1691076 Fe 1.2620E+03 BCC_A2 0.9731763 5.3674E+02 FCC_A1 0.7329179 Gibbs Energy = -5.6600073645E+07 J System Enthalpy = 3.0458723499E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 773.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 773.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.3175E+03 BCC_A2 0.0002132 0.0072612 0.0182899 4.8118E+02 FCC_A1 0.0343675 0.0748406 0.1885137 Fe 1.3175E+03 BCC_A2 0.9742356 4.8118E+02 FCC_A1 0.7022782 Gibbs Energy = -5.4426884904E+07 J System Enthalpy = 2.8731888452E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 753.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 753.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.3638E+03 BCC_A2 0.0002141 0.0068953 0.0173683 4.3492E+02 FCC_A1 0.0379972 0.0831754 0.2095079 Fe 1.3638E+03 BCC_A2 0.9755223 4.3492E+02 FCC_A1 0.6693195 Gibbs Energy = -5.2297650555E+07 J System Enthalpy = 2.7059220190E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 733.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 733.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.4025E+03 BCC_A2 0.0002129 0.0064777 0.0163164 3.9616E+02 FCC_A1 0.0416990 0.0921187 0.2320348 Fe 1.4025E+03 BCC_A2 0.9769930 3.9616E+02 FCC_A1 0.6341475 Gibbs Energy = -5.0212175933E+07 J System Enthalpy = 2.5435371609E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 713.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 713.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.4352E+03 BCC_A2 0.0002087 0.0060225 0.0151700 3.6353E+02 FCC_A1 0.0454387 0.1016016 0.2559210 Fe 1.4352E+03 BCC_A2 0.9785987 3.6353E+02 FCC_A1 0.5970387 Gibbs Energy = -4.8170372782E+07 J System Enthalpy = 2.3857018262E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 693.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 693.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.4627E+03 BCC_A2 0.0002007 0.0055447 0.0139663 3.3602E+02 FCC_A1 0.0491767 0.1115064 0.2808700 Fe 1.4627E+03 BCC_A2 0.9802884 3.3602E+02 FCC_A1 0.5584469 Gibbs Energy = -4.6172218770E+07 J System Enthalpy = 2.2322315227E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 673.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 673.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.4859E+03 BCC_A2 0.0001877 0.0050581 0.0127406 3.1282E+02 FCC_A1 0.0528711 0.1216781 0.3064910 Fe 1.4859E+03 BCC_A2 0.9820136 3.1282E+02 FCC_A1 0.5189598 Gibbs Energy = -4.4217729916E+07 J System Enthalpy = 2.0830241606E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 653.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 653.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5055E+03 BCC_A2 0.0001695 0.0045748 0.0115233 2.9324E+02 FCC_A1 0.0564824 0.1319462 0.3323551 Fe 1.5055E+03 BCC_A2 0.9837324 2.9324E+02 FCC_A1 0.4792163 Gibbs Energy = -4.2306949016E+07 J System Enthalpy = 1.9379991271E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 633.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 633.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5220E+03 BCC_A2 0.0001466 0.0041042 0.0103380 2.7669E+02 FCC_A1 0.0599757 0.1421505 0.3580584 Fe 1.5220E+03 BCC_A2 0.9854111 2.7669E+02 FCC_A1 0.4398153 Gibbs Energy = -4.0439948323E+07 J System Enthalpy = 1.7970578633E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 613.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 613.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5360E+03 BCC_A2 0.0001204 0.0036532 0.0092018 2.6267E+02 FCC_A1 0.0633225 0.1521572 0.3832640 Fe 1.5360E+03 BCC_A2 0.9870246 2.6267E+02 FCC_A1 0.4012563 Gibbs Energy = -3.8616840470E+07 J System Enthalpy = 1.6600727263E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 593.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 593.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5480E+03 BCC_A2 0.0000933 0.0032260 0.0081258 2.5074E+02 FCC_A1 0.0664984 0.1618640 0.4077141 Fe 1.5480E+03 BCC_A2 0.9885550 2.5074E+02 FCC_A1 0.3639235 Gibbs Energy = -3.6837790999E+07 J System Enthalpy = 1.5268943874E+07 J *** PROBLEM settings *** Changes only listed under components/phases/substances NUMBER COMPONENT STATUS AMOUNT DELTA REF.P NUMBER PHASE STATUS MODEL NUMBER SUBSTANCE STATUS/CONSTRAINT TEMPERATURE : 573.1500 PRESSURE/Pa : 101325.0 VOLUME/m3 : undefined SYSTEM AMOUNT/mol : undefined COMP. AMOUNTS/mol : 16.81792 45.57865 114.8066 1621.502 SYSTEM MASS/kg : 100.0000 COMP. MASSES/kg : 0.2020000 2.504000 6.738000 90.55600 STEPPED VARIABLE INITIAL, FINAL AND STEP VALUES OF VARIABLE TEMPERATURE 993.150 to 573.150 by -20.0000 *** MULTIPHASE - Stage 1* Results *** Temperature = 573.1500 K Fixed pressure = 1.013250E+05 Pa, 1.000000E+00 atm Component Ref.Phase Chem.Pot. Activity Amount/mol Mass/kg C undef undef 1.681792E+01 2.020000E-01 Mn undef undef 4.557865E+01 2.504000E+00 Ni undef undef 1.148066E+02 6.738000E+00 Fe undef undef 1.621502E+03 9.055600E+01 Total 1.798705E+03 1.000000E+02 Amount Phase Mole fraction of component within phase compnt moles C Mn Ni 1.5582E+03 BCC_A2 0.0000678 0.0028253 0.0071165 2.4052E+02 FCC_A1 0.0694837 0.1711961 0.4312205 Fe 1.5582E+03 BCC_A2 0.9899904 2.4052E+02 FCC_A1 0.3280997 Gibbs Energy = -3.5103028966E+07 J System Enthalpy = 1.3973637067E+07 J