Calculations using MTTTDATA, http://www.msm.cam.ac.uk/map/steel/programs/MTTTDATA.html Weldox ------ WEIGHT % Fe= 94.0000 Cr= 0.7000 Co= 0.0000 Ni= 2.0000 Mo= 0.7000 Mn= 1.6000 Si= 0.5000 Al= 0.0000 Cu= 0.3000 V= 0.0000 Nb= 0.0000 C= 0.2000 MOL FRACTION Fe= 0.9318 Cr= 0.0075 Co= 0.0000 Ni= 0.0189 Mo= 0.0040 Mn= 0.0161 Si= 0.0099 Al= 0.0000 Cu= 0.0026 V= 0.0000 Nb= 0.0000 C= 0.0092 TEMP, GN, GMAX, FPRO, FTO, X NUCLEUS, XEQ, XA, XW , XTO, XTO400, VOLF, SHEART, DIFFT 473. -2400. -3169. -2691. -2570. 0.11E-05 0.1996 0.13E-03 0.1752 0.0654 0.0570 0.9544 0.48E+05 0.16E+18 483. -2355. -3088. -2782. -2664. 0.11E-05 0.1965 0.15E-03 0.1721 0.0642 0.0557 0.9538 0.24E+05 0.24E+17 493. -2310. -3007. -2703. -2587. 0.11E-05 0.1934 0.17E-03 0.1689 0.0630 0.0545 0.9532 0.12E+05 0.38E+16 503. -2265. -2927. -2625. -2511. 0.11E-05 0.1903 0.19E-03 0.1658 0.0618 0.0532 0.9525 0.65E+04 0.67E+15 513. -2221. -2847. -2547. -2435. 0.11E-05 0.1871 0.21E-03 0.1626 0.0605 0.0519 0.9518 0.36E+04 0.13E+15 523. -2176. -2767. -2469. -2360. 0.11E-05 0.1839 0.23E-03 0.1594 0.0593 0.0506 0.9511 0.21E+04 0.26E+14 533. -2131. -2688. -2393. -2285. 0.11E-05 0.1807 0.26E-03 0.1561 0.0580 0.0493 0.9503 0.13E+04 0.58E+13 543. -2086. -2609. -2316. -2210. 0.11E-05 0.1774 0.28E-03 0.1528 0.0568 0.0480 0.9496 0.81E+03 0.14E+13 553. -2042. -2530. -2240. -2136. 0.11E-05 0.1741 0.31E-03 0.1495 0.0555 0.0466 0.9487 0.53E+03 0.35E+12 563. -1997. -2452. -2165. -2062. 0.11E-05 0.1708 0.33E-03 0.1462 0.0542 0.0453 0.9479 0.35E+03 0.96E+11 573. -1952. -2375. -2090. -1988. 0.11E-05 0.1674 0.36E-03 0.1428 0.0529 0.0440 0.9470 0.24E+03 0.27E+11 583. -1907. -2298. -2016. -1916. 0.11E-05 0.1640 0.39E-03 0.1394 0.0516 0.0426 0.9460 0.17E+03 0.83E+10 593. -1863. -2221. -1942. -1843. 0.11E-05 0.1606 0.42E-03 0.1360 0.0503 0.0412 0.9451 0.13E+03 0.27E+10 603. -1818. -2145. -1869. -1772. 0.11E-05 0.1571 0.45E-03 0.1325 0.0490 0.0399 0.9440 0.97E+02 0.90E+09 613. -1773. -2070. -1797. -1701. 0.11E-05 0.1536 0.48E-03 0.1290 0.0477 0.0385 0.9429 0.75E+02 0.32E+09 623. -1728. -1995. -1725. -1630. 0.11E-05 0.1500 0.50E-03 0.1254 0.0464 0.0371 0.9417 0.60E+02 0.12E+09 633. -1684. -1921. -1654. -1560. 0.11E-05 0.1464 0.53E-03 0.1219 0.0451 0.0357 0.9405 0.49E+02 0.46E+08 643. -1639. -1848. -1584. -1491. 0.11E-05 0.1428 0.56E-03 0.1183 0.0437 0.0343 0.9391 0.41E+02 0.18E+08 653. -1594. -1775. -1515. -1422. 0.30E-05 0.1391 0.59E-03 0.1146 0.0424 0.0330 0.9377 0.35E+02 0.78E+07 663. -1549. -1703. -1446. -1354. 0.36E-05 0.1354 0.61E-03 0.1110 0.0410 0.0315 0.9362 0.30E+02 0.34E+07 673. -1505. -1632. -1379. -1287. 0.43E-05 0.1317 0.64E-03 0.1073 0.0397 0.0301 0.9345 0.27E+02 0.15E+07 683. -1460. -1561. -1312. -1221. 0.51E-05 0.1279 0.66E-03 0.1036 0.0384 0.0287 0.9327 0.25E+02 0.73E+06 693. -1415. -1492. -1246. -1155. 0.60E-05 0.1241 0.68E-03 0.0998 0.0370 0.0273 0.9308 0.23E+02 0.36E+06 703. -1370. -1423. -1181. -1091. 0.71E-05 0.1202 0.70E-03 0.0961 0.0357 0.0259 0.9287 0.22E+02 0.18E+06 713. -1326. -1355. -1117. -1027. 0.84E-05 0.1163 0.72E-03 0.0923 0.0343 0.0244 0.9265 0.22E+02 0.94E+05 723. -1281. -1288. -1054. -964. 0.98E-05 0.1124 0.74E-03 0.0884 0.0330 0.0230 0.9240 0.21E+02 0.51E+05 733. -1236. -1222. -993. -902. 0.11E-04 0.1084 0.75E-03 0.0846 0.0316 0.0216 0.9214 0.22E+02 0.28E+05 743. -1191. -1156. -932. -841. 0.13E-04 0.1044 0.76E-03 0.0808 0.0303 0.0202 0.9184 0.23E+02 0.16E+05 753. -1147. -1092. -872. -781. 0.15E-04 0.1004 0.77E-03 0.0769 0.0289 0.0188 0.9152 0.24E+02 0.97E+04 763. -1102. -1029. -814. -721. 0.18E-04 0.0963 0.78E-03 0.0730 0.0276 0.0173 0.9117 0.26E+02 0.59E+04 773. -1057. -967. -757. -663. 0.20E-04 0.0922 0.78E-03 0.0691 0.0262 0.0159 0.9077 0.29E+02 0.37E+04 783. -1012. -906. -701. -606. 0.23E-04 0.0881 0.79E-03 0.0652 0.0249 0.0145 0.9034 0.33E+02 0.24E+04 793. -968. -846. -647. -551. 0.26E-04 0.0839 0.78E-03 0.0613 0.0236 0.0131 0.8986 0.39E+02 0.16E+04 803. -923. -788. -593. -496. 0.30E-04 0.0798 0.78E-03 0.0574 0.0223 0.0117 0.8931 0.47E+02 0.11E+04 813. -878. -730. -542. -443. 0.34E-04 0.0756 0.77E-03 0.0535 0.0210 0.0103 0.8871 0.58E+02 0.78E+03 823. -833. -674. -492. -390. 0.38E-04 0.0713 0.76E-03 0.0497 0.0197 0.0090 0.8802 0.73E+02 0.57E+03 833. -789. -619. -443. -340. 0.43E-04 0.0671 0.75E-03 0.0458 0.0184 0.0076 0.8723 0.96E+02 0.43E+03 843. -744. -566. -396. -290. 0.48E-04 0.0629 0.73E-03 0.0420 0.0171 0.0062 0.8634 0.13E+03 0.33E+03 853. -699. -514. -351. -242. 0.54E-04 0.0586 0.71E-03 0.0383 0.0159 0.0049 0.8531 0.18E+03 0.27E+03 863. -654. -463. -308. -195. 0.60E-04 0.0544 0.68E-03 0.0345 0.0146 0.0036 0.8412 0.27E+03 0.22E+03 873. -610. -414. -267. -150. 0.66E-04 0.0502 0.66E-03 0.0309 0.0134 0.0023 0.8272 0.42E+03 0.19E+03 883. -565. -367. -228. -107. 0.74E-04 0.0460 0.63E-03 0.0273 0.0122 0.0010 0.8106 0.68E+03 0.18E+03 893. -520. -321. -190. -65. 0.81E-04 0.0418 0.59E-03 0.0239 0.0111 0.0000 0.7909 0.12E+04 0.17E+03 903. -475. -277. -156. -24. 0.90E-04 0.0377 0.55E-03 0.0205 0.0099 0.0000 0.7669 0.22E+04 0.17E+03 913. -431. -234. -124. 14. 0.99E-04 0.0337 0.51E-03 0.0173 0.0088 0.0000 0.7374 0.46E+04 0.18E+03 923. -386. -194. -94. 51. 0.11E-03 0.0297 0.47E-03 0.0142 0.0077 0.0000 0.7004 0.11E+05 0.21E+03 933. -341. -155. -68. 86. 0.12E-03 0.0258 0.43E-03 0.0113 0.0067 0.0000 0.6531 0.30E+05 0.28E+03 943. -296. -119. -45. 119. 0.13E-03 0.0220 0.38E-03 0.0086 0.0057 0.0000 0.5907 0.10E+06 0.42E+03 953. -252. -84. -26. 150. 0.14E-03 0.0183 0.33E-03 0.0062 0.0047 0.0000 0.5058 0.53E+06 0.82E+03 963. -207. -52. -11. 178. 0.15E-03 0.0148 0.28E-03 0.0040 0.0038 0.0000 0.3847 0.55E+07 0.24E+04 973. -162. -22. -2. 205. 0.17E-03 0.0115 0.22E-03 0.0022 0.0030 0.0000 0.2009 0.39E+09 0.23E+05 MS= 643. K BS= 733. K WS1= 733. K WS2= 0. K WS3= 0. K OK7578 ------ WEIGHT % Fe= 93.6600 Cr= 0.4000 Co= 0.0000 Ni= 3.1000 Mo= 0.6000 Mn= 2.0000 Si= 0.1900 Al= 0.0000 Cu= 0.0000 V= 0.0000 Nb= 0.0000 C= 0.0500 MOL FRACTION Fe= 0.9363 Cr= 0.0043 Co= 0.0000 Ni= 0.0295 Mo= 0.0035 Mn= 0.0203 Si= 0.0038 Al= 0.0000 Cu= 0.0000 V= 0.0000 Nb= 0.0000 C= 0.0023 TEMP, GN, GMAX, FPRO, FTO, X NUCLEUS, XEQ, XA, XW , XTO, XTO400, VOLF, SHEART, DIFFT 473. -2400. -3035. -2946. -2926. 0.11E-05 0.1939 0.10E-03 0.1694 0.0618 0.0534 0.9885 0.60E+05 0.18E+18 483. -2355. -2956. -2867. -2848. 0.11E-05 0.1908 0.12E-03 0.1663 0.0606 0.0522 0.9884 0.29E+05 0.27E+17 493. -2310. -2876. -2788. -2770. 0.11E-05 0.1876 0.13E-03 0.1631 0.0594 0.0509 0.9883 0.15E+05 0.43E+16 503. -2265. -2797. -2709. -2692. 0.11E-05 0.1844 0.15E-03 0.1599 0.0582 0.0496 0.9882 0.82E+04 0.76E+15 513. -2221. -2719. -2631. -2614. 0.11E-05 0.1812 0.17E-03 0.1567 0.0569 0.0483 0.9881 0.46E+04 0.15E+15 523. -2176. -2640. -2553. -2537. 0.11E-05 0.1780 0.19E-03 0.1534 0.0557 0.0470 0.9880 0.27E+04 0.30E+14 533. -2131. -2563. -2476. -2460. 0.11E-05 0.1747 0.21E-03 0.1501 0.0544 0.0457 0.9879 0.16E+04 0.67E+13 543. -2086. -2485. -2399. -2384. 0.11E-05 0.1714 0.23E-03 0.1467 0.0532 0.0444 0.9877 0.10E+04 0.16E+13 553. -2042. -2408. -2322. -2308. 0.11E-05 0.1680 0.25E-03 0.1434 0.0519 0.0431 0.9876 0.67E+03 0.41E+12 563. -1997. -2332. -2246. -2232. 0.11E-05 0.1646 0.27E-03 0.1400 0.0506 0.0418 0.9875 0.45E+03 0.11E+12 573. -1952. -2256. -2170. -2157. 0.11E-05 0.1612 0.29E-03 0.1365 0.0493 0.0404 0.9874 0.32E+03 0.32E+11 583. -1907. -2180. -2096. -2083. 0.11E-05 0.1577 0.32E-03 0.1330 0.0480 0.0391 0.9872 0.23E+03 0.97E+10 593. -1863. -2105. -2021. -2009. 0.11E-05 0.1542 0.34E-03 0.1295 0.0467 0.0377 0.9871 0.17E+03 0.31E+10 603. -1818. -2031. -1947. -1935. 0.11E-05 0.1506 0.36E-03 0.1260 0.0454 0.0363 0.9869 0.13E+03 0.11E+10 613. -1773. -1957. -1874. -1863. 0.11E-05 0.1470 0.38E-03 0.1224 0.0441 0.0350 0.9868 0.99E+02 0.38E+09 623. -1728. -1884. -1802. -1791. 0.11E-05 0.1433 0.41E-03 0.1188 0.0428 0.0337 0.9866 0.80E+02 0.14E+09 633. -1684. -1811. -1730. -1719. 0.11E-05 0.1397 0.43E-03 0.1151 0.0415 0.0322 0.9864 0.65E+02 0.54E+08 643. -1639. -1739. -1659. -1648. 0.11E-05 0.1359 0.45E-03 0.1114 0.0401 0.0308 0.9862 0.55E+02 0.22E+08 653. -1594. -1668. -1588. -1578. 0.11E-05 0.1322 0.47E-03 0.1077 0.0388 0.0294 0.9859 0.47E+02 0.94E+07 663. -1549. -1598. -1519. -1509. 0.11E-05 0.1284 0.49E-03 0.1040 0.0375 0.0280 0.9857 0.42E+02 0.41E+07 673. -1505. -1528. -1450. -1440. 0.11E-05 0.1245 0.51E-03 0.1002 0.0361 0.0266 0.9854 0.38E+02 0.19E+07 683. -1460. -1459. -1382. -1372. 0.11E-05 0.1206 0.53E-03 0.0964 0.0348 0.0252 0.9851 0.35E+02 0.89E+06 693. -1415. -1391. -1314. -1305. 0.11E-05 0.1167 0.55E-03 0.0926 0.0334 0.0238 0.9847 0.33E+02 0.44E+06 703. -1370. -1324. -1248. -1239. 0.11E-05 0.1127 0.56E-03 0.0887 0.0321 0.0224 0.9843 0.32E+02 0.22E+06 713. -1326. -1257. -1183. -1174. 0.11E-05 0.1087 0.57E-03 0.0848 0.0307 0.0209 0.9838 0.31E+02 0.12E+06 723. -1281. -1192. -1118. -1109. 0.11E-05 0.1046 0.58E-03 0.0809 0.0294 0.0195 0.9833 0.32E+02 0.64E+05 733. -1236. -1127. -1055. -1046. 0.28E-05 0.1005 0.59E-03 0.0769 0.0280 0.0181 0.9827 0.33E+02 0.36E+05 743. -1191. -1064. -992. -983. 0.32E-05 0.0964 0.60E-03 0.0730 0.0267 0.0167 0.9820 0.35E+02 0.21E+05 753. -1147. -1001. -931. -922. 0.37E-05 0.0922 0.61E-03 0.0690 0.0254 0.0153 0.9812 0.37E+02 0.13E+05 763. -1102. -940. -870. -861. 0.42E-05 0.0880 0.61E-03 0.0650 0.0240 0.0139 0.9804 0.41E+02 0.77E+04 773. -1057. -879. -811. -802. 0.48E-05 0.0837 0.61E-03 0.0610 0.0227 0.0125 0.9793 0.47E+02 0.49E+04 783. -1012. -820. -753. -744. 0.55E-05 0.0794 0.60E-03 0.0570 0.0214 0.0111 0.9782 0.55E+02 0.32E+04 793. -968. -762. -696. -687. 0.63E-05 0.0751 0.60E-03 0.0530 0.0201 0.0097 0.9768 0.66E+02 0.22E+04 803. -923. -705. -640. -631. 0.71E-05 0.0707 0.59E-03 0.0490 0.0187 0.0083 0.9753 0.81E+02 0.15E+04 813. -878. -650. -586. -576. 0.80E-05 0.0663 0.58E-03 0.0450 0.0175 0.0069 0.9735 0.10E+03 0.11E+04 823. -833. -595. -533. -523. 0.91E-05 0.0619 0.56E-03 0.0411 0.0162 0.0056 0.9713 0.14E+03 0.82E+03 833. -789. -542. -482. -471. 0.10E-04 0.0575 0.55E-03 0.0371 0.0149 0.0042 0.9688 0.19E+03 0.64E+03 843. -744. -491. -432. -420. 0.11E-04 0.0531 0.52E-03 0.0332 0.0136 0.0029 0.9657 0.27E+03 0.51E+03 853. -699. -440. -383. -371. 0.13E-04 0.0486 0.50E-03 0.0294 0.0124 0.0015 0.9621 0.40E+03 0.43E+03 863. -654. -392. -336. -323. 0.14E-04 0.0442 0.47E-03 0.0256 0.0112 0.0002 0.9576 0.63E+03 0.37E+03 873. -610. -344. -291. -277. 0.16E-04 0.0397 0.44E-03 0.0220 0.0101 0.0000 0.9521 0.10E+04 0.34E+03 883. -565. -299. -248. -232. 0.17E-04 0.0353 0.41E-03 0.0184 0.0088 0.0000 0.9451 0.19E+04 0.33E+03 893. -520. -255. -207. -189. 0.19E-04 0.0309 0.37E-03 0.0150 0.0077 0.0000 0.9360 0.37E+04 0.34E+03 903. -475. -213. -167. -148. 0.21E-04 0.0265 0.33E-03 0.0117 0.0065 0.0000 0.9240 0.83E+04 0.37E+03 913. -431. -172. -130. -109. 0.24E-04 0.0223 0.29E-03 0.0087 0.0054 0.0000 0.9073 0.21E+05 0.46E+03 923. -386. -134. -96. -71. 0.26E-04 0.0180 0.24E-03 0.0058 0.0044 0.0000 0.8830 0.68E+05 0.65E+03 933. -341. -97. -64. -36. 0.28E-04 0.0139 0.20E-03 0.0034 0.0034 0.0000 0.8447 0.31E+06 0.11E+04 943. -296. -63. -36. -2. 0.31E-04 0.0099 0.14E-03 0.0013 0.0024 0.0000 0.7766 0.25E+07 0.29E+04 953. -252. -30. -12. 29. 0.34E-04 0.0060 0.92E-04 0.0000 0.0014 0.0000 0.6246 0.86E+08 0.17E+05 963. -207. 0. 0. 59. 0.37E-04 0.0024 0.37E-04 0.0000 0.0006 0.0000 0.0118 0.15E+19 0.17E+11 MS= 673. K BS= 683. K WS1= 683. K WS2= 0. K WS3= 0. K OK7478 diluted with Weldox -------------------------- WEIGHT % Fe= 93.8300 Cr= 0.5500 Co= 0.0000 Ni= 2.5500 Mo= 0.6500 Mn= 1.8000 Si= 0.3450 Al= 0.0000 Cu= 0.1500 V= 0.0000 Nb= 0.0000 C= 0.1250 MOL FRACTION Fe= 0.9341 Cr= 0.0059 Co= 0.0000 Ni= 0.0242 Mo= 0.0038 Mn= 0.0182 Si= 0.0068 Al= 0.0000 Cu= 0.0013 V= 0.0000 Nb= 0.0000 C= 0.0058 TEMP, GN, GMAX, FPRO, FTO, X NUCLEUS, XEQ, XA, XW , XTO, XTO400, VOLF, SHEART, DIFFT 473. -2400. -3100. -2791. -2724. 0.11E-05 0.1967 0.11E-03 0.1722 0.0636 0.0552 0.9711 0.54E+05 0.17E+18 483. -2355. -3019. -2817. -2752. 0.11E-05 0.1936 0.13E-03 0.1691 0.0624 0.0539 0.9708 0.26E+05 0.25E+17 493. -2310. -2939. -2739. -2674. 0.11E-05 0.1905 0.15E-03 0.1659 0.0611 0.0526 0.9704 0.14E+05 0.41E+16 503. -2265. -2859. -2660. -2597. 0.11E-05 0.1873 0.17E-03 0.1628 0.0599 0.0514 0.9700 0.73E+04 0.72E+15 513. -2221. -2780. -2582. -2521. 0.11E-05 0.1841 0.19E-03 0.1596 0.0587 0.0501 0.9696 0.41E+04 0.14E+15 523. -2176. -2701. -2504. -2444. 0.11E-05 0.1809 0.21E-03 0.1563 0.0574 0.0488 0.9691 0.24E+04 0.28E+14 533. -2131. -2622. -2427. -2368. 0.11E-05 0.1776 0.23E-03 0.1530 0.0562 0.0475 0.9687 0.15E+04 0.63E+13 543. -2086. -2544. -2350. -2293. 0.11E-05 0.1743 0.25E-03 0.1497 0.0549 0.0461 0.9682 0.92E+03 0.15E+13 553. -2042. -2467. -2274. -2218. 0.11E-05 0.1710 0.28E-03 0.1464 0.0536 0.0448 0.9677 0.60E+03 0.38E+12 563. -1997. -2389. -2198. -2143. 0.11E-05 0.1676 0.30E-03 0.1430 0.0524 0.0435 0.9672 0.40E+03 0.10E+12 573. -1952. -2312. -2123. -2069. 0.11E-05 0.1642 0.33E-03 0.1396 0.0511 0.0421 0.9667 0.28E+03 0.30E+11 583. -1907. -2236. -2048. -1995. 0.11E-05 0.1608 0.35E-03 0.1361 0.0498 0.0408 0.9661 0.20E+03 0.90E+10 593. -1863. -2161. -1974. -1922. 0.11E-05 0.1573 0.38E-03 0.1327 0.0485 0.0394 0.9655 0.15E+03 0.29E+10 603. -1818. -2085. -1901. -1850. 0.11E-05 0.1538 0.40E-03 0.1291 0.0472 0.0380 0.9649 0.11E+03 0.98E+09 613. -1773. -2011. -1828. -1778. 0.11E-05 0.1502 0.43E-03 0.1256 0.0459 0.0367 0.9642 0.87E+02 0.35E+09 623. -1728. -1937. -1756. -1706. 0.11E-05 0.1466 0.45E-03 0.1220 0.0445 0.0353 0.9635 0.69E+02 0.13E+09 633. -1684. -1864. -1684. -1636. 0.11E-05 0.1430 0.48E-03 0.1184 0.0432 0.0339 0.9627 0.57E+02 0.50E+08 643. -1639. -1791. -1614. -1566. 0.11E-05 0.1393 0.50E-03 0.1148 0.0419 0.0325 0.9619 0.47E+02 0.20E+08 653. -1594. -1719. -1544. -1496. 0.11E-05 0.1356 0.53E-03 0.1111 0.0405 0.0311 0.9610 0.41E+02 0.86E+07 663. -1549. -1648. -1475. -1428. 0.11E-05 0.1318 0.55E-03 0.1074 0.0392 0.0297 0.9601 0.36E+02 0.38E+07 673. -1505. -1577. -1406. -1360. 0.26E-05 0.1280 0.57E-03 0.1037 0.0378 0.0283 0.9591 0.32E+02 0.17E+07 683. -1460. -1508. -1339. -1293. 0.31E-05 0.1242 0.59E-03 0.0999 0.0365 0.0269 0.9580 0.30E+02 0.81E+06 693. -1415. -1439. -1272. -1227. 0.37E-05 0.1203 0.61E-03 0.0961 0.0352 0.0255 0.9567 0.28E+02 0.40E+06 703. -1370. -1371. -1207. -1161. 0.44E-05 0.1164 0.63E-03 0.0923 0.0338 0.0241 0.9554 0.27E+02 0.20E+06 713. -1326. -1304. -1142. -1096. 0.51E-05 0.1124 0.64E-03 0.0884 0.0325 0.0226 0.9540 0.26E+02 0.11E+06 723. -1281. -1237. -1078. -1033. 0.60E-05 0.1084 0.66E-03 0.0846 0.0311 0.0212 0.9524 0.26E+02 0.57E+05 733. -1236. -1172. -1016. -970. 0.70E-05 0.1044 0.67E-03 0.0807 0.0298 0.0198 0.9506 0.27E+02 0.32E+05 743. -1191. -1108. -954. -908. 0.81E-05 0.1003 0.68E-03 0.0768 0.0284 0.0184 0.9487 0.28E+02 0.19E+05 753. -1147. -1044. -893. -847. 0.94E-05 0.0962 0.68E-03 0.0728 0.0271 0.0170 0.9466 0.30E+02 0.11E+05 763. -1102. -982. -834. -788. 0.11E-04 0.0920 0.69E-03 0.0689 0.0257 0.0155 0.9442 0.33E+02 0.68E+04 773. -1057. -921. -776. -729. 0.12E-04 0.0879 0.69E-03 0.0650 0.0244 0.0141 0.9415 0.37E+02 0.43E+04 783. -1012. -861. -719. -671. 0.14E-04 0.0837 0.69E-03 0.0610 0.0231 0.0127 0.9386 0.43E+02 0.28E+04 793. -968. -802. -663. -615. 0.16E-04 0.0794 0.68E-03 0.0571 0.0217 0.0113 0.9352 0.51E+02 0.19E+04 803. -923. -744. -609. -560. 0.18E-04 0.0751 0.68E-03 0.0531 0.0204 0.0099 0.9314 0.62E+02 0.13E+04 813. -878. -687. -556. -506. 0.21E-04 0.0709 0.67E-03 0.0492 0.0191 0.0086 0.9271 0.78E+02 0.93E+03 823. -833. -632. -505. -453. 0.23E-04 0.0665 0.65E-03 0.0453 0.0178 0.0072 0.9221 0.10E+03 0.69E+03 833. -789. -578. -455. -402. 0.26E-04 0.0622 0.64E-03 0.0414 0.0166 0.0058 0.9164 0.14E+03 0.53E+03 843. -744. -526. -407. -351. 0.29E-04 0.0579 0.62E-03 0.0375 0.0153 0.0045 0.9098 0.19E+03 0.42E+03 853. -699. -475. -360. -303. 0.33E-04 0.0535 0.60E-03 0.0337 0.0141 0.0031 0.9020 0.27E+03 0.34E+03 863. -654. -425. -315. -256. 0.36E-04 0.0492 0.57E-03 0.0300 0.0128 0.0018 0.8927 0.42E+03 0.29E+03 873. -610. -377. -272. -210. 0.41E-04 0.0449 0.54E-03 0.0263 0.0116 0.0005 0.8817 0.67E+03 0.26E+03 883. -565. -330. -231. -166. 0.45E-04 0.0406 0.51E-03 0.0227 0.0104 0.0000 0.8682 0.11E+04 0.24E+03 893. -520. -285. -192. -123. 0.50E-04 0.0363 0.47E-03 0.0193 0.0093 0.0000 0.8516 0.21E+04 0.24E+03 903. -475. -242. -156. -83. 0.55E-04 0.0320 0.43E-03 0.0159 0.0081 0.0000 0.8307 0.43E+04 0.25E+03 913. -431. -201. -122. -44. 0.60E-04 0.0279 0.39E-03 0.0128 0.0070 0.0000 0.8036 0.99E+04 0.29E+03 923. -386. -161. -91. -7. 0.66E-04 0.0238 0.35E-03 0.0098 0.0060 0.0000 0.7677 0.27E+05 0.37E+03 933. -341. -124. -62. 29. 0.73E-04 0.0197 0.30E-03 0.0070 0.0049 0.0000 0.7179 0.92E+05 0.55E+03 943. -296. -88. -38. 62. 0.79E-04 0.0158 0.25E-03 0.0046 0.0040 0.0000 0.6451 0.46E+06 0.10E+04 953. -252. -55. -18. 93. 0.87E-04 0.0121 0.20E-03 0.0024 0.0030 0.0000 0.5300 0.45E+07 0.30E+04 963. -207. -24. -4. 122. 0.94E-04 0.0085 0.15E-03 0.0008 0.0021 0.0000 0.3240 0.28E+09 0.26E+05 MS= 663. K BS= 713. K WS1= 713. K WS2= 0. K WS3= 0. K LTTE ---- WEIGHT % Fe= 80.8300 Cr= 9.1000 Co= 0.0000 Ni= 8.5000 Mo= 0.0000 Mn= 1.3000 Si= 0.2000 Al= 0.0000 Cu= 0.0000 V= 0.0000 Nb= 0.0000 C= 0.0700 MOL FRACTION Fe= 0.8024 Cr= 0.0970 Co= 0.0000 Ni= 0.0803 Mo= 0.0000 Mn= 0.0131 Si= 0.0039 Al= 0.0000 Cu= 0.0000 V= 0.0000 Nb= 0.0000 C= 0.0032 TEMP, GN, GMAX, FPRO, FTO, X NUCLEUS, XEQ, XA, XW , XTO, XTO400, VOLF, SHEART, DIFFT 473. -2400. -2068. -1970. -1961. 0.11E-05 0.1665 0.74E-03 0.1402 0.0584 0.0468 0.9850 0.41E+06 0.58E+18 483. -2355. -1999. -1902. -1894. 0.11E-05 0.1630 0.78E-03 0.1367 0.0568 0.0451 0.9849 0.21E+06 0.87E+17 493. -2310. -1931. -1835. -1826. 0.11E-05 0.1593 0.82E-03 0.1330 0.0552 0.0435 0.9848 0.11E+06 0.14E+17 503. -2265. -1862. -1767. -1759. 0.11E-05 0.1557 0.86E-03 0.1294 0.0535 0.0418 0.9847 0.62E+05 0.26E+16 513. -2221. -1795. -1700. -1692. 0.11E-05 0.1520 0.90E-03 0.1257 0.0519 0.0401 0.9846 0.37E+05 0.51E+15 523. -2176. -1727. -1634. -1626. 0.11E-05 0.1482 0.93E-03 0.1220 0.0503 0.0384 0.9844 0.22E+05 0.11E+15 533. -2131. -1660. -1567. -1560. 0.11E-05 0.1444 0.97E-03 0.1182 0.0486 0.0367 0.9842 0.14E+05 0.25E+14 543. -2086. -1594. -1502. -1495. 0.11E-05 0.1406 0.10E-02 0.1144 0.0470 0.0350 0.9840 0.95E+04 0.61E+13 553. -2042. -1527. -1437. -1430. 0.11E-05 0.1366 0.10E-02 0.1105 0.0453 0.0333 0.9837 0.66E+04 0.16E+13 563. -1997. -1462. -1372. -1365. 0.11E-05 0.1327 0.10E-02 0.1066 0.0437 0.0316 0.9834 0.47E+04 0.45E+12 573. -1952. -1397. -1308. -1301. 0.11E-05 0.1286 0.11E-02 0.1026 0.0420 0.0299 0.9830 0.35E+04 0.13E+12 583. -1907. -1332. -1244. -1237. 0.29E-05 0.1245 0.11E-02 0.0986 0.0403 0.0281 0.9826 0.27E+04 0.43E+11 593. -1863. -1268. -1181. -1174. 0.34E-05 0.1204 0.11E-02 0.0946 0.0387 0.0264 0.9821 0.21E+04 0.14E+11 603. -1818. -1204. -1119. -1112. 0.40E-05 0.1162 0.11E-02 0.0905 0.0370 0.0247 0.9815 0.17E+04 0.51E+10 613. -1773. -1142. -1057. -1050. 0.47E-05 0.1119 0.11E-02 0.0863 0.0353 0.0229 0.9808 0.15E+04 0.19E+10 623. -1728. -1079. -996. -989. 0.54E-05 0.1076 0.11E-02 0.0822 0.0336 0.0212 0.9800 0.13E+04 0.74E+09 633. -1684. -1018. -936. -928. 0.63E-05 0.1032 0.11E-02 0.0779 0.0320 0.0194 0.9791 0.12E+04 0.31E+09 643. -1639. -957. -876. -869. 0.72E-05 0.0987 0.11E-02 0.0737 0.0303 0.0177 0.9780 0.11E+04 0.13E+09 653. -1594. -897. -817. -809. 0.83E-05 0.0942 0.11E-02 0.0693 0.0286 0.0160 0.9768 0.11E+04 0.60E+08 663. -1549. -837. -759. -751. 0.95E-05 0.0895 0.11E-02 0.0650 0.0269 0.0142 0.9754 0.11E+04 0.29E+08 673. -1505. -778. -702. -693. 0.11E-04 0.0849 0.10E-02 0.0606 0.0252 0.0125 0.9737 0.11E+04 0.14E+08 683. -1460. -720. -645. -636. 0.12E-04 0.0801 0.10E-02 0.0562 0.0236 0.0107 0.9718 0.12E+04 0.74E+07 693. -1415. -663. -590. -580. 0.14E-04 0.0753 0.96E-03 0.0517 0.0219 0.0090 0.9695 0.13E+04 0.41E+07 703. -1370. -607. -535. -525. 0.16E-04 0.0704 0.92E-03 0.0473 0.0202 0.0072 0.9668 0.16E+04 0.23E+07 713. -1326. -552. -482. -471. 0.18E-04 0.0654 0.88E-03 0.0428 0.0186 0.0055 0.9635 0.19E+04 0.14E+07 723. -1281. -497. -429. -417. 0.20E-04 0.0603 0.83E-03 0.0383 0.0169 0.0038 0.9596 0.25E+04 0.88E+06 733. -1236. -444. -378. -365. 0.22E-04 0.0551 0.78E-03 0.0338 0.0153 0.0021 0.9549 0.35E+04 0.59E+06 743. -1191. -391. -328. -313. 0.24E-04 0.0499 0.72E-03 0.0293 0.0137 0.0004 0.9489 0.51E+04 0.42E+06 753. -1147. -340. -279. -263. 0.27E-04 0.0446 0.65E-03 0.0248 0.0120 0.0000 0.9413 0.83E+04 0.32E+06 763. -1102. -289. -232. -214. 0.30E-04 0.0392 0.59E-03 0.0204 0.0104 0.0000 0.9315 0.15E+05 0.26E+06 773. -1057. -240. -186. -165. 0.33E-04 0.0337 0.51E-03 0.0161 0.0088 0.0000 0.9180 0.31E+05 0.24E+06 783. -1012. -192. -142. -118. 0.36E-04 0.0281 0.43E-03 0.0119 0.0073 0.0000 0.8989 0.78E+05 0.25E+06 793. -968. -145. -101. -72. 0.40E-04 0.0224 0.35E-03 0.0079 0.0057 0.0000 0.8696 0.26E+06 0.32E+06 803. -923. -99. -62. -27. 0.43E-04 0.0167 0.27E-03 0.0043 0.0042 0.0000 0.8191 0.15E+07 0.55E+06 813. -878. -55. -27. 16. 0.47E-04 0.0108 0.17E-03 0.0013 0.0027 0.0000 0.7126 0.24E+08 0.18E+07 823. -833. -12. -2. 58. 0.52E-04 0.0049 0.80E-04 0.0000 0.0012 0.0000 0.3419 0.48E+11 0.11E+09 MS= 553. K BS= 473. K WS1= 473. K WS2= 0. K WS3= 0. K LTTE Diluted with Weldox ------------------------ WEIGHT % Fe= 87.7650 Cr= 4.9000 Co= 0.0000 Ni= 5.2500 Mo= 0.0000 Mn= 1.4500 Si= 0.3500 Al= 0.0000 Cu= 0.1500 V= 0.0000 Nb= 0.0000 C= 0.1350 MOL FRACTION Fe= 0.8694 Cr= 0.0521 Co= 0.0000 Ni= 0.0495 Mo= 0.0000 Mn= 0.0146 Si= 0.0069 Al= 0.0000 Cu= 0.0013 V= 0.0000 Nb= 0.0000 C= 0.0062 TEMP, GN, GMAX, FPRO, FTO, X NUCLEUS, XEQ, XA, XW , XTO, XTO400, VOLF, SHEART, DIFFT 473. -2400. -2562. -2234. -2183. 0.11E-05 0.1828 0.30E-03 0.1574 0.0613 0.0515 0.9676 0.14E+06 0.30E+18 483. -2355. -2488. -2294. -2244. 0.11E-05 0.1795 0.33E-03 0.1541 0.0599 0.0501 0.9672 0.70E+05 0.45E+17 493. -2310. -2413. -2221. -2172. 0.11E-05 0.1762 0.36E-03 0.1507 0.0585 0.0486 0.9667 0.36E+05 0.73E+16 503. -2265. -2339. -2148. -2100. 0.11E-05 0.1728 0.40E-03 0.1473 0.0571 0.0472 0.9662 0.20E+05 0.13E+16 513. -2221. -2266. -2076. -2029. 0.11E-05 0.1694 0.43E-03 0.1439 0.0557 0.0457 0.9657 0.11E+05 0.25E+15 523. -2176. -2192. -2004. -1958. 0.11E-05 0.1659 0.46E-03 0.1404 0.0543 0.0442 0.9652 0.68E+04 0.53E+14 533. -2131. -2119. -1933. -1888. 0.11E-05 0.1624 0.49E-03 0.1369 0.0529 0.0427 0.9646 0.42E+04 0.12E+14 543. -2086. -2047. -1862. -1818. 0.11E-05 0.1588 0.52E-03 0.1334 0.0514 0.0413 0.9640 0.27E+04 0.29E+13 553. -2042. -1975. -1792. -1748. 0.11E-05 0.1552 0.55E-03 0.1298 0.0500 0.0398 0.9634 0.18E+04 0.74E+12 563. -1997. -1903. -1722. -1679. 0.11E-05 0.1516 0.58E-03 0.1262 0.0485 0.0382 0.9627 0.13E+04 0.20E+12 573. -1952. -1832. -1653. -1611. 0.11E-05 0.1479 0.61E-03 0.1225 0.0471 0.0367 0.9620 0.89E+03 0.60E+11 583. -1907. -1762. -1585. -1543. 0.11E-05 0.1442 0.64E-03 0.1188 0.0456 0.0352 0.9612 0.66E+03 0.18E+11 593. -1863. -1692. -1517. -1475. 0.11E-05 0.1404 0.67E-03 0.1151 0.0441 0.0337 0.9603 0.50E+03 0.60E+10 603. -1818. -1623. -1449. -1408. 0.11E-05 0.1366 0.70E-03 0.1113 0.0427 0.0321 0.9594 0.39E+03 0.21E+10 613. -1773. -1554. -1383. -1342. 0.29E-05 0.1327 0.72E-03 0.1075 0.0412 0.0306 0.9584 0.31E+03 0.75E+09 623. -1728. -1486. -1317. -1276. 0.35E-05 0.1288 0.74E-03 0.1036 0.0397 0.0291 0.9572 0.26E+03 0.29E+09 633. -1684. -1418. -1252. -1211. 0.41E-05 0.1248 0.76E-03 0.0998 0.0382 0.0275 0.9560 0.22E+03 0.11E+09 643. -1639. -1351. -1187. -1147. 0.49E-05 0.1208 0.78E-03 0.0958 0.0367 0.0260 0.9547 0.19E+03 0.47E+08 653. -1594. -1285. -1123. -1083. 0.58E-05 0.1168 0.79E-03 0.0919 0.0352 0.0244 0.9532 0.17E+03 0.20E+08 663. -1549. -1220. -1061. -1020. 0.68E-05 0.1127 0.81E-03 0.0879 0.0337 0.0228 0.9516 0.16E+03 0.93E+07 673. -1505. -1155. -999. -958. 0.79E-05 0.1085 0.82E-03 0.0839 0.0322 0.0213 0.9498 0.15E+03 0.44E+07 683. -1460. -1091. -938. -896. 0.92E-05 0.1043 0.82E-03 0.0798 0.0308 0.0197 0.9478 0.15E+03 0.21E+07 693. -1415. -1028. -877. -835. 0.11E-04 0.1000 0.82E-03 0.0757 0.0293 0.0181 0.9456 0.15E+03 0.11E+07 703. -1370. -966. -818. -776. 0.12E-04 0.0957 0.82E-03 0.0716 0.0278 0.0166 0.9431 0.15E+03 0.58E+06 713. -1326. -905. -760. -717. 0.14E-04 0.0913 0.82E-03 0.0674 0.0263 0.0150 0.9403 0.16E+03 0.32E+06 723. -1281. -844. -703. -659. 0.16E-04 0.0869 0.81E-03 0.0633 0.0248 0.0135 0.9372 0.18E+03 0.18E+06 733. -1236. -785. -647. -602. 0.18E-04 0.0824 0.80E-03 0.0591 0.0233 0.0119 0.9336 0.20E+03 0.11E+06 743. -1191. -726. -592. -545. 0.21E-04 0.0779 0.79E-03 0.0549 0.0219 0.0104 0.9295 0.23E+03 0.66E+05 753. -1147. -669. -538. -490. 0.24E-04 0.0733 0.77E-03 0.0507 0.0204 0.0088 0.9248 0.28E+03 0.42E+05 763. -1102. -613. -486. -436. 0.27E-04 0.0686 0.74E-03 0.0464 0.0189 0.0073 0.9194 0.35E+03 0.28E+05 773. -1057. -557. -435. -383. 0.30E-04 0.0640 0.72E-03 0.0422 0.0174 0.0057 0.9130 0.46E+03 0.19E+05 783. -1012. -503. -385. -331. 0.33E-04 0.0592 0.69E-03 0.0380 0.0160 0.0042 0.9055 0.63E+03 0.14E+05 793. -968. -450. -337. -281. 0.37E-04 0.0545 0.65E-03 0.0339 0.0146 0.0027 0.8966 0.92E+03 0.11E+05 803. -923. -398. -291. -231. 0.42E-04 0.0497 0.61E-03 0.0297 0.0131 0.0012 0.8857 0.14E+04 0.85E+04 813. -878. -348. -246. -183. 0.46E-04 0.0448 0.57E-03 0.0256 0.0117 0.0000 0.8723 0.24E+04 0.72E+04 823. -833. -298. -203. -136. 0.51E-04 0.0399 0.52E-03 0.0216 0.0104 0.0000 0.8555 0.43E+04 0.65E+04 833. -789. -251. -162. -90. 0.56E-04 0.0350 0.47E-03 0.0177 0.0090 0.0000 0.8337 0.89E+04 0.65E+04 843. -744. -204. -124. -46. 0.62E-04 0.0301 0.42E-03 0.0139 0.0076 0.0000 0.8045 0.21E+05 0.71E+04 853. -699. -159. -89. -3. 0.68E-04 0.0251 0.36E-03 0.0103 0.0063 0.0000 0.7636 0.65E+05 0.90E+04 863. -654. -116. -56. 38. 0.75E-04 0.0202 0.30E-03 0.0069 0.0050 0.0000 0.7024 0.28E+06 0.14E+05 873. -610. -74. -29. 78. 0.82E-04 0.0153 0.23E-03 0.0039 0.0038 0.0000 0.6015 0.23E+07 0.35E+05 883. -565. -33. -8. 116. 0.89E-04 0.0103 0.16E-03 0.0013 0.0025 0.0000 0.4048 0.11E+09 0.24E+06 MS= 603. K BS= 533. K WS1= 533. K WS2= 0. K WS3= 0. K Series B -------- WEIGHT % Fe= 85.3200 Cr= 1.0000 Co= 0.0000 Ni= 12.0000 Mo= 0.5000 Mn= 0.5000 Si= 0.6500 Al= 0.0000 Cu= 0.0000 V= 0.0000 Nb= 0.0000 C= 0.0300 MOL FRACTION Fe= 0.8528 Cr= 0.0107 Co= 0.0000 Ni= 0.1141 Mo= 0.0029 Mn= 0.0051 Si= 0.0129 Al= 0.0000 Cu= 0.0000 V= 0.0000 Nb= 0.0000 C= 0.0014 TEMP, GN, GMAX, FPRO, FTO, X NUCLEUS, XEQ, XA, XW , XTO, XTO400, VOLF, SHEART, DIFFT 473. -2400. -1825. -1779. -1763. 0.11E-05 0.1541 0.31E-04 0.1278 0.0387 0.0301 0.9911 0.76E+06 0.84E+18 483. -2355. -1753. -1708. -1692. 0.11E-05 0.1502 0.35E-04 0.1239 0.0375 0.0288 0.9909 0.40E+06 0.13E+18 493. -2310. -1682. -1637. -1622. 0.11E-05 0.1462 0.40E-04 0.1200 0.0362 0.0275 0.9907 0.22E+06 0.22E+17 503. -2265. -1611. -1566. -1552. 0.11E-05 0.1421 0.45E-04 0.1159 0.0350 0.0262 0.9905 0.13E+06 0.40E+16 513. -2221. -1541. -1496. -1482. 0.11E-05 0.1380 0.50E-04 0.1119 0.0337 0.0249 0.9903 0.78E+05 0.80E+15 523. -2176. -1471. -1426. -1412. 0.11E-05 0.1338 0.56E-04 0.1077 0.0324 0.0235 0.9900 0.50E+05 0.17E+15 533. -2131. -1401. -1357. -1343. 0.11E-05 0.1296 0.61E-04 0.1035 0.0311 0.0222 0.9897 0.33E+05 0.41E+14 543. -2086. -1332. -1288. -1275. 0.11E-05 0.1252 0.67E-04 0.0992 0.0298 0.0208 0.9894 0.23E+05 0.10E+14 553. -2042. -1263. -1220. -1207. 0.11E-05 0.1208 0.73E-04 0.0949 0.0285 0.0194 0.9891 0.17E+05 0.28E+13 563. -1997. -1195. -1152. -1139. 0.11E-05 0.1163 0.78E-04 0.0905 0.0272 0.0180 0.9887 0.13E+05 0.83E+12 573. -1952. -1127. -1084. -1072. 0.11E-05 0.1117 0.84E-04 0.0860 0.0258 0.0166 0.9883 0.10E+05 0.26E+12 583. -1907. -1060. -1018. -1005. 0.11E-05 0.1070 0.89E-04 0.0815 0.0245 0.0152 0.9878 0.84E+04 0.85E+11 593. -1863. -993. -952. -939. 0.11E-05 0.1022 0.93E-04 0.0769 0.0231 0.0138 0.9873 0.72E+04 0.30E+11 603. -1818. -927. -886. -874. 0.11E-05 0.0973 0.97E-04 0.0722 0.0218 0.0124 0.9867 0.64E+04 0.11E+11 613. -1773. -862. -821. -809. 0.11E-05 0.0923 0.10E-03 0.0674 0.0204 0.0110 0.9860 0.60E+04 0.44E+10 623. -1728. -797. -757. -745. 0.11E-05 0.0872 0.10E-03 0.0626 0.0191 0.0095 0.9852 0.59E+04 0.18E+10 633. -1684. -733. -694. -682. 0.11E-05 0.0820 0.11E-03 0.0577 0.0177 0.0081 0.9843 0.60E+04 0.82E+09 643. -1639. -670. -631. -619. 0.11E-05 0.0766 0.11E-03 0.0527 0.0163 0.0066 0.9832 0.65E+04 0.39E+09 653. -1594. -607. -570. -557. 0.11E-05 0.0711 0.11E-03 0.0477 0.0149 0.0052 0.9819 0.74E+04 0.19E+09 663. -1549. -546. -509. -496. 0.11E-05 0.0655 0.10E-03 0.0426 0.0135 0.0037 0.9803 0.90E+04 0.10E+09 673. -1505. -484. -449. -435. 0.11E-05 0.0597 0.10E-03 0.0374 0.0121 0.0023 0.9783 0.12E+05 0.59E+08 683. -1460. -424. -390. -376. 0.11E-05 0.0538 0.98E-04 0.0322 0.0107 0.0008 0.9758 0.17E+05 0.36E+08 693. -1415. -365. -331. -317. 0.11E-05 0.0476 0.92E-04 0.0269 0.0093 0.0000 0.9726 0.26E+05 0.24E+08 703. -1370. -306. -274. -259. 0.11E-05 0.0413 0.84E-04 0.0217 0.0080 0.0000 0.9682 0.48E+05 0.18E+08 713. -1326. -249. -219. -202. 0.11E-05 0.0347 0.74E-04 0.0165 0.0066 0.0000 0.9619 0.10E+06 0.15E+08 723. -1281. -192. -164. -146. 0.11E-05 0.0279 0.63E-04 0.0114 0.0052 0.0000 0.9522 0.29E+06 0.15E+08 733. -1236. -137. -112. -91. 0.26E-05 0.0209 0.49E-04 0.0065 0.0038 0.0000 0.9354 0.13E+07 0.20E+08 743. -1191. -82. -61. -37. 0.29E-05 0.0135 0.33E-04 0.0022 0.0024 0.0000 0.8988 0.13E+08 0.46E+08 753. -1147. -28. -16. 16. 0.34E-05 0.0057 0.14E-04 0.0000 0.0010 0.0000 0.7590 0.20E+10 0.55E+09 MS= 523. K BS= 473. K WS1= 473. K WS2= 0. K WS3= 0. K Series B diluted with Weldox ---------------------------- WEIGHT % Fe= 89.6600 Cr= 0.8500 Co= 0.0000 Ni= 7.0000 Mo= 0.6000 Mn= 1.0500 Si= 0.5750 Al= 0.0000 Cu= 0.1500 V= 0.0000 Nb= 0.0000 C= 0.1150 MOL FRACTION Fe= 0.8925 Cr= 0.0091 Co= 0.0000 Ni= 0.0663 Mo= 0.0035 Mn= 0.0106 Si= 0.0114 Al= 0.0000 Cu= 0.0013 V= 0.0000 Nb= 0.0000 C= 0.0053 TEMP, GN, GMAX, FPRO, FTO, X NUCLEUS, XEQ, XA, XW , XTO, XTO400, VOLF, SHEART, DIFFT 473. -2400. -2519. -2233. -2161. 0.11E-05 0.1802 0.67E-04 0.1549 0.0527 0.0442 0.9708 0.15E+06 0.32E+18 483. -2355. -2443. -2273. -2203. 0.11E-05 0.1768 0.77E-04 0.1515 0.0515 0.0429 0.9703 0.76E+05 0.48E+17 493. -2310. -2367. -2198. -2130. 0.11E-05 0.1734 0.87E-04 0.1480 0.0502 0.0416 0.9698 0.40E+05 0.78E+16 503. -2265. -2291. -2124. -2056. 0.11E-05 0.1699 0.99E-04 0.1445 0.0490 0.0403 0.9692 0.22E+05 0.14E+16 513. -2221. -2216. -2050. -1984. 0.11E-05 0.1664 0.11E-03 0.1410 0.0477 0.0390 0.9687 0.13E+05 0.27E+15 523. -2176. -2141. -1976. -1911. 0.11E-05 0.1628 0.12E-03 0.1375 0.0465 0.0377 0.9680 0.77E+04 0.57E+14 533. -2131. -2066. -1903. -1839. 0.11E-05 0.1592 0.14E-03 0.1338 0.0452 0.0364 0.9674 0.48E+04 0.13E+14 543. -2086. -1992. -1830. -1767. 0.11E-05 0.1556 0.15E-03 0.1302 0.0439 0.0351 0.9667 0.31E+04 0.31E+13 553. -2042. -1919. -1758. -1696. 0.11E-05 0.1519 0.16E-03 0.1265 0.0427 0.0337 0.9660 0.21E+04 0.81E+12 563. -1997. -1846. -1686. -1625. 0.11E-05 0.1481 0.18E-03 0.1228 0.0414 0.0324 0.9652 0.15E+04 0.22E+12 573. -1952. -1773. -1615. -1555. 0.11E-05 0.1443 0.19E-03 0.1190 0.0401 0.0310 0.9644 0.11E+04 0.66E+11 583. -1907. -1701. -1545. -1486. 0.11E-05 0.1404 0.21E-03 0.1152 0.0388 0.0296 0.9635 0.79E+03 0.21E+11 593. -1863. -1629. -1475. -1416. 0.11E-05 0.1365 0.22E-03 0.1113 0.0374 0.0283 0.9626 0.60E+03 0.68E+10 603. -1818. -1558. -1406. -1348. 0.11E-05 0.1326 0.24E-03 0.1074 0.0361 0.0269 0.9616 0.48E+03 0.23E+10 613. -1773. -1488. -1337. -1280. 0.11E-05 0.1286 0.25E-03 0.1034 0.0348 0.0255 0.9605 0.39E+03 0.86E+09 623. -1728. -1418. -1270. -1213. 0.11E-05 0.1245 0.26E-03 0.0994 0.0334 0.0241 0.9593 0.33E+03 0.33E+09 633. -1684. -1349. -1203. -1146. 0.11E-05 0.1203 0.28E-03 0.0954 0.0321 0.0227 0.9580 0.28E+03 0.13E+09 643. -1639. -1281. -1136. -1080. 0.11E-05 0.1162 0.29E-03 0.0913 0.0308 0.0213 0.9566 0.25E+03 0.55E+08 653. -1594. -1213. -1071. -1015. 0.11E-05 0.1119 0.30E-03 0.0872 0.0294 0.0198 0.9550 0.23E+03 0.24E+08 663. -1549. -1146. -1006. -950. 0.11E-05 0.1076 0.31E-03 0.0830 0.0281 0.0184 0.9533 0.22E+03 0.11E+08 673. -1505. -1080. -943. -886. 0.30E-05 0.1032 0.32E-03 0.0788 0.0267 0.0170 0.9514 0.21E+03 0.53E+07 683. -1460. -1015. -880. -823. 0.35E-05 0.0988 0.33E-03 0.0745 0.0253 0.0156 0.9493 0.21E+03 0.27E+07 693. -1415. -950. -818. -761. 0.42E-05 0.0943 0.33E-03 0.0703 0.0240 0.0141 0.9469 0.22E+03 0.14E+07 703. -1370. -886. -757. -700. 0.49E-05 0.0897 0.34E-03 0.0659 0.0226 0.0127 0.9442 0.24E+03 0.75E+06 713. -1326. -824. -697. -639. 0.58E-05 0.0851 0.34E-03 0.0616 0.0212 0.0113 0.9412 0.26E+03 0.42E+06 723. -1281. -762. -639. -580. 0.67E-05 0.0804 0.34E-03 0.0572 0.0199 0.0098 0.9377 0.30E+03 0.25E+06 733. -1236. -701. -581. -521. 0.78E-05 0.0756 0.34E-03 0.0528 0.0185 0.0084 0.9338 0.35E+03 0.15E+06 743. -1191. -641. -525. -464. 0.90E-05 0.0708 0.33E-03 0.0483 0.0172 0.0069 0.9291 0.44E+03 0.96E+05 753. -1147. -582. -470. -407. 0.10E-04 0.0659 0.33E-03 0.0439 0.0158 0.0055 0.9237 0.56E+03 0.64E+05 763. -1102. -524. -416. -352. 0.12E-04 0.0609 0.32E-03 0.0394 0.0145 0.0041 0.9173 0.77E+03 0.45E+05 773. -1057. -468. -364. -297. 0.14E-04 0.0558 0.30E-03 0.0349 0.0131 0.0027 0.9096 0.11E+04 0.33E+05 783. -1012. -412. -313. -244. 0.16E-04 0.0507 0.29E-03 0.0305 0.0118 0.0012 0.9001 0.17E+04 0.26E+05 793. -968. -358. -264. -192. 0.18E-04 0.0455 0.27E-03 0.0261 0.0104 0.0000 0.8882 0.29E+04 0.21E+05 803. -923. -304. -217. -141. 0.20E-04 0.0402 0.25E-03 0.0217 0.0091 0.0000 0.8730 0.54E+04 0.19E+05 813. -878. -253. -172. -92. 0.23E-04 0.0348 0.23E-03 0.0174 0.0078 0.0000 0.8528 0.12E+05 0.19E+05 823. -833. -202. -129. -43. 0.25E-04 0.0294 0.20E-03 0.0133 0.0065 0.0000 0.8247 0.30E+05 0.21E+05 833. -789. -153. -89. 3. 0.28E-04 0.0239 0.17E-03 0.0093 0.0052 0.0000 0.7831 0.11E+06 0.28E+05 843. -744. -105. -53. 49. 0.32E-04 0.0184 0.13E-03 0.0056 0.0040 0.0000 0.7155 0.59E+06 0.52E+05 853. -699. -59. -22. 93. 0.36E-04 0.0127 0.96E-04 0.0024 0.0027 0.0000 0.5869 0.94E+07 0.18E+06 863. -654. -14. -2. 136. 0.39E-04 0.0071 0.55E-04 0.0001 0.0015 0.0000 0.2490 0.11E+11 0.82E+07 MS= 593. K BS= 513. K WS1= 513. K WS2= 0. K WS3= 0. K